Preparation method of alumina pellets with large specific surface area and large pore volume
High-purity alumina spheres are prepared by combining rotating liquid membrane reactor with template induced crystallization, which solves the problem of insufficient specific surface area and pore capacity of the catalyst support in the prior art, and realizes oxidation with large specific surface area and rich pore structure Aluminum pellets are suitable for catalytic reactions in the field of refining and chemical industry.
Patent Information
- Application Number
- CN202411224941.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The prior art is difficult to prepare alumina catalyst support with high specific surface area and large pore volume in the field of refining and chemical engineering, resulting in insufficient catalytic reaction activity, and the collapse of the pore structure of the template-induced crystallization method leads to a decrease in the specific surface area, affecting the catalytic activity of the catalyst.
The method of combining rotary liquid film reactor and template induced crystallization is adopted to prepare high-purity large specific surface area and large pore volume suprasite through hydrolysis of aluminum alcohol, and alumina spheres are prepared by oil column molding, using EO20PO10EO20 as Template inducers control crystal growth and pore structure.
Improve the specific surface area and pore structure of alumina spheres, enhance the loading performance and dispersion of active components, and is suitable for oxidation, dehydrogenation, reforming and other reactions in the petrochemical field, especially for continuous reforming and propane Dehydrogenation.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of alumina pellets, and in particular relates to a method for preparing alumina pellets with large specific surface area and large pore volume. Background Art
[0002] As a widely used chemical product, activated alumina is widely used as a catalyst carrier due to its suitable specific surface area, rich pore volume and pore size, and good chemical stability. At present, in the chemical industry, especially in petrochemical and biochemical industries, high molecular weight raw materials are increasingly used, which requires the catalyst or catalyst carrier used to have larger mesopores or macropores and larger specific surface area. Therefore, the study of appropriate improvement of the pore structure of activated alumina has become a hot topic.
[0003] Patent CN1160602A discloses a large-pore alumina carrier and its preparation method, with a pore volume of 0.80-1.20 mL / g and a specific surface area of 110-200 m 2 / g. During the kneading process of pseudo-boehmite and water or aqueous solution, physical pore expanders such as carbon black and chemical pore expanders such as phosphorus compounds are added at the same time. The specific surface area of the alumina carrier produced by this method still needs to be further improved. Patent CN104353502A discloses a method for preparing macroporous spherical alumina, wherein aluminum colloid, water, and alginate solution are evenly mixed, pseudo-boehmite or alumina powder is added, and a suspension slurry is made by high-speed stirring, and then dripped into a multivalent metal cation aqueous solution to form gel spheres, which are dried and calcined after molding to obtain the product. However, the addition of metal cation aqueous solution may introduce other impurity ions, resulting in a decrease in the purity of alumina. Patent CN103172097A discloses a method for preparing pseudo-boehmite, wherein aluminate solution and aluminum salt solution are simultaneously poured into a rotating liquid film reactor for rapid mixing and nucleation, and the pseudo-boehmite is prepared into a catalyst after molding and carrying active components, which can be widely used in catalytic hydrogenation reactions.
[0004] In the field of petroleum refining and chemical industry, with the deterioration and heaviness of crude oil, alumina with high specific surface area and large pore volume is increasingly needed as a catalyst carrier to increase the internal diffusion rate, promote the transfer of long-chain molecules, and improve the catalytic reaction activity. The spatial structure of the material synthesized by the template-induced crystallization method depends on the structural orientation of the template agent, which causes the skeleton and pore structure to change. Some template agents cause the collapse of the pore structure of pseudo-boehmite during peptization and heat treatment. Therefore, it is necessary to obtain a template inducer with improved crystal order to achieve a balance between the basic physical properties and reaction performance of the porous material. In addition, the expansion of the pore structure of the synthesized pseudo-boehmite will inevitably lead to a decrease in the specific surface area, which is not conducive to the uniform dispersion of the active phase, thereby affecting the catalytic activity of the catalyst. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing alumina beads by applying a rotating liquid film reactor combined with template-induced crystallization to synthesize high-purity, large specific surface area, and large pore volume pseudo-boehmite by alcohol aluminum hydrolysis method. The alumina beads prepared by this method have the characteristics of high specific surface area, rich pore structure, high crushing strength and good stability. The high specific surface area is conducive to providing more active sites, increasing the contact between the active sites and the reactants, and improving the reaction rate; the large pore volume is conducive to improving the dispersibility of the metal catalytic active center, and providing the required pores for the diffusion of the metal active center in the subsequent preparation of the supported solid catalyst. The loading performance is improved by expanding the pore structure and specific surface area, and the dispersibility of the active components is improved. The alumina beads are suitable for oxidation, dehydrogenation, reforming, polymerization and other reaction processes in the field of petrochemical industry, and are particularly suitable for continuous reforming, propane dehydrogenation and other reactions.
[0006] To achieve the above object, the present invention adopts the following technical solution: A method for preparing alumina spheres with large specific surface area and large pore volume, the method is specifically as follows: (a) adding aluminum alcoholate and an organic solvent to a rotating liquid film reactor at the same time, mixing, setting the temperature, and stirring to dissolve the aluminum alcoholate; (b) adding deionized water and a template inducing agent to the alcohol aluminum organic solution prepared in step (a), and stirring for a certain period of time to allow the solution to react fully; (c) transferring the mixed slurry of step (b) to a hydrothermal crystallization reactor for crystal growth, and setting a specific temperature and time for the crystallization reaction; (d) after the crystallization is completed, the material is discharged, filtered, and dried to a constant weight to obtain pseudo-boehmite powder; (e) dissolving the pseudo-boehmite obtained in step (d) in water to obtain a pseudo-boehmite suspension, and adding an acid solution for peptization; (f) adding a curing agent to the aluminum sol prepared in step (e); (g) dropping the slurry obtained in step (f) into a hot oil column to form spherical gel particles; (h) The gel beads obtained in step (g) are taken out and subjected to aging, washing, drying and calcination to obtain alumina beads.
[0007] Preferably, the aluminum alcoholate in (a) is one or more of aluminum methoxide, aluminum ethoxide, aluminum isopropoxide, aluminum sec-butoxide, aluminum n-hexoxide and aluminum isooctoxide; Preferably, the organic solvent in (a) is one of isopropanol, n-butanol, sec-butanol, n-pentanol, n-hexanol and tetrahydrofuran; Preferably, the molar ratio of the aluminum alcoholate to the organic solvent in (a) is 1:2-6; Preferably, the dissolving temperature in (a) is 60-100°C and the stirring speed is 300-600 rpm; Preferably, the molar ratio of the aluminum alcoholate to deionized water in (b) is 1:2-6; the stirring time of the rotating liquid film reactor is set to 10 min-2 h; Preferably, the template inducing agent in (b) is EO 20 PO 10 EO 20 ; Preferably, the crystallization temperature in (c) is 100-160°C and the crystallization time is 4-14 h; Preferably, the drying temperature in (d) is 80-120°C; Preferably, the mass percentage of aluminum oxide in the pseudo-boehmite suspension in (e) is 5-30%; Preferably, the mass ratio of the acid solution to the aluminum oxide in the pseudo-boehmite suspension in (e) is 0.1-1, and the pH is controlled at 2-5; the acid solution is one of the aqueous solutions of nitric acid, hydrochloric acid, sulfuric acid or formic acid with a mass percentage concentration of 3-30%; Preferably, the mass ratio of the curing agent to the aluminum oxide in the aluminum sol in (f) is 0.2-0.6; the curing agent is hexamethylenetetramine, urea or a mixture of the two; Preferably, the molding oil in the hot oil column in (g) is one of vacuum pump oil, machine oil, white oil, spindle oil, and mineral oil; Preferably, the oil column temperature in (g) is 90-99°C; Preferably, the aging temperature in (h) is 120-180°C, and the aging time is 12-48 h; the drying temperature is 50-100°C, and the drying time is 12-24 h; the roasting temperature is 550-1050°C, and the roasting time is 3-6 h.
[0008] The advantages of the present invention are: The method uses a rotating liquid film reactor combined with a template-induced crystallization method to hydrolyze alcohol aluminum to prepare pseudo-boehmite, and uses oil column molding to prepare alumina spheres. The rotating liquid film reactor promotes rapid and large-scale nucleation of solid and liquid at high shear speed, increases the solid-liquid contact area, and improves the specific surface area of pseudo-boehmite; EO 20 PO 10 EO 20As a template inducer with large molecular weight, regular and stable structure, it will spontaneously and orderly aggregate to form micelles in aqueous solution. After the aluminum source is hydrolyzed in the solution, it will self-assemble along the outer surface of the micelles. The template-induced crystallization controls the morphology of crystal growth and regulates the size of the crystal, which promotes the improvement of crystal order and uniform distribution of grains. After crystallization treatment, a stable and orderly mesoporous structure is formed. The alumina beads obtained from the powder obtained by this method have the characteristics of expanding the pore structure and specific surface area, improving the loading performance, and improving the dispersion of active components.
[0009] This method uses a rotating liquid film reactor combined with template-induced crystallization to complete the hydrolysis of aluminum isopropoxide. A large number of nuclei are promoted at high shear rates, which prevents the occurrence of nucleation during the aging process, increases the solid-liquid contact area, and improves the specific surface area of pseudo-boehmite. Compared with pore-enlarging agents such as DMF and DMHA, the use of EO 20 PO 10 EO 20 Template-induced crystallization controls the morphology of crystal growth and regulates the size of crystals, which can improve the order of crystals and evenly distribute grains. Pseudo-boehmite with large pore structure and specific surface area and uniform grains was obtained. Alumina spheres prepared by oil column molding have large specific surface area and pore structure. It is suitable for oxidation, dehydrogenation, reforming, polymerization and other reaction processes in the petrochemical field, especially for continuous reforming, propane dehydrogenation and other reactions. DETAILED DESCRIPTION
[0010] In order to make the above features and advantages of the present invention more clearly understood, the following embodiments are given for detailed description. The methods of the present invention are all conventional methods in the art unless otherwise specified.
[0011] Example 1 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them into a rotating liquid film reactor. Set the temperature to 80 °C and the speed to 300 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Add 5 g of EO 20 PO 10 EO 20 Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to the rotating liquid film reactor at a set flow rate of 20 g / h, maintain the temperature at 80 °C, and continue stirring for 30 minutes after the water is added. Transfer the mixed slurry to the hydrothermal crystallization reactor and crystallize at 120 °C for 4 hours. The crystallized slurry is filtered and dried at 120 °C for 12 hours until the product quality no longer changes, and the pseudo-boehmite sample PB-1 is obtained.
[0012] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-1, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then use a dispersed dropper to drip into an oil column filled with vacuum pump oil at 90 °C to form. Separate the formed gel balls from the oil and age them in an aging kettle at 140 °C for 10 hours. Wash the aged sol balls, then dry them at 60 °C for 12 hours to constant weight, and then calcine them at 650 °C for 5 hours to obtain aluminum oxide balls SALO-1.
[0013] Example 2 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them into a rotating liquid film reactor. Set the temperature to 80 °C and the speed to 600 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Add 5 g of EO 20 PO 10 EO 20 Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to the rotating liquid film reactor at a set flow rate of 20 g / h, maintain the temperature at 80 °C, and continue stirring for 1 h after the addition of water. Transfer the mixed slurry to a hydrothermal crystallization reactor and crystallize at 120 °C for 4 h. The crystallized slurry is filtered and dried at 120 °C for 12 h until the product quality no longer changes, and the pseudo-boehmite sample PB-2 is obtained.
[0014] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-2, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then use a dispersed dropper to drip into an oil column filled with vacuum pump oil at 90 ° C to form, separate the formed gel beads from the oil, and age them in an aging kettle at 140 ° C for 10 hours. Wash the aged sol balls, then dry them at 60 ° C for 12 hours to constant weight, and then calcine them at 650 ° C for 5 hours to obtain aluminum oxide beads SALO-2.
[0015] Example 3 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them into a rotating liquid film reactor. Set the temperature to 80 °C and the speed to 300 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Add 5 g of EO 20 PO 10 EO 20Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to the rotating liquid film reactor at a set flow rate of 20 g / h, maintain the temperature at 80 °C, and continue stirring for 30 minutes after the water is added. Transfer the mixed slurry to the hydrothermal crystallization reactor and crystallize at 140 °C for 4 hours. The crystallized slurry is filtered and dried at 120 °C for 12 hours until the product quality no longer changes, and the pseudo-boehmite sample PB-3 is obtained.
[0016] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-3, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then drip it into an oil column filled with vacuum pump oil at 90 ℃ with a dispersing dropper to form it. Separate the formed gel balls from the oil and age them in an aging kettle at 140 ℃ for 10 hours. Wash the aged sol balls, then dry them at 60 ℃ for 12 hours to constant weight, and then calcine them at 650 ℃ for 5 hours to obtain aluminum oxide balls SALO-3.
[0017] Example 4 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them into a rotating liquid film reactor. Set the temperature to 80 °C and the speed to 600 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Add 5 g of EO 20 PO 10 EO 20 Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to the rotating liquid film reactor at a set flow rate of 20 g / h, maintain the temperature at 80 °C, and continue stirring for 1 h after the addition of water. Transfer the mixed slurry to a hydrothermal crystallization reactor and crystallize at 140 °C for 4 h. The crystallized slurry is filtered and dried at 120 °C for 12 h until the product quality no longer changes, and the pseudo-boehmite sample PB-4 is obtained.
[0018] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-4, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then use a dispersed dropper to drip into an oil column filled with vacuum pump oil at 90 ° C to form. Separate the formed gel balls from the oil and age them in an aging kettle at 140 ° C for 10 hours. Wash the aged sol balls, then dry them at 60 ° C for 12 hours to constant weight, and then calcine them at 650 ° C for 5 hours to obtain aluminum oxide balls SALO-4.
[0019] Example 5 A. Take 60 g of aluminum isopropoxide and 80 g of isopropanol and add them into a rotating liquid film reactor. Set the temperature to 80 °C and the speed to 600 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Add 7.5 g of EO 20 PO 10 EO 20 Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to the rotating liquid film reactor at a set flow rate of 20 g / h, maintain the temperature at 80 °C, and continue stirring for 30 minutes after the water is added. Transfer the mixed slurry to the hydrothermal crystallization reactor and crystallize at 140 °C for 4 hours. The crystallized slurry is filtered and dried at 120 °C for 12 hours until the product quality no longer changes, and the pseudo-boehmite sample PB-5 is obtained.
[0020] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-5, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then drip it into an oil column filled with vacuum pump oil at 90 ℃ with a dispersing dropper to form it. Separate the formed gel balls from the oil and age them in an aging kettle at 140 ℃ for 10 hours. Wash the aged sol balls, then dry them at 60 ℃ for 12 hours to constant weight, and then calcine them at 650 ℃ for 5 hours to obtain aluminum oxide balls SALO-5.
[0021] Comparative Example 1 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them to a three-necked flask and place it in an 80°C oil bath. Stir mechanically to dissolve the aluminum isopropoxide. 20 PO 10 EO 20 Dissolve in 25 g of deionized water to obtain a mixed solution, and use a peristaltic pump to add it to a three-necked flask at a set flow rate of 20 g / h, keep the temperature at 80 °C, and continue stirring for 30 minutes after the water is added. Transfer the mixed slurry to a hydrothermal crystallization reactor and age at 120 °C for 4 h. Filter the crystallized slurry and dry it at 120 °C for 12 h until the product quality no longer changes, and obtain the pseudo-boehmite sample CPB-1.
[0022] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite CPB-1, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2-5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then use a dispersed dropper to drip into an oil column filled with vacuum pump oil at 90 ° C to form. Separate the formed gel balls from the oil and age them in an aging kettle at 140 ° C for 10 hours. Wash the aged sol balls, then dry them at 60 ° C for 12 hours to constant weight, and then calcine them at 650 ° C for 5 hours to obtain alumina balls CSALO-1.
[0023] Comparative Example 2 A. Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them to the rotating liquid film reactor. Set the temperature to 80 °C and the speed to 300 rpm. Run for 1 h to completely dissolve the aluminum isopropoxide. Mix 5 g of DMF and 25 g of deionized water and add them to the rotating liquid film reactor at a set flow rate of 20 g / h using a peristaltic pump. Keep the temperature at 80 °C and continue stirring for 30 min after adding water. Transfer the mixed slurry to the hydrothermal crystallization reactor and crystallize at 120 °C for 4 h. The crystallized slurry is filtered and dried at 120 °C for 12 h until the product quality no longer changes, and the pseudo-boehmite sample CPB-2 is obtained.
[0024] B. Take 10 g of the above-mentioned self-made 100-mesh sieved pseudo-boehmite PB-1, add 30 g of deionized water and 1.5 g of 20 wt% nitric acid solution and stir continuously to obtain aluminum sol (pH 2~5). Add 1 g of 35 wt% hexamethylenetetramine solution to the aluminum sol, stir and mix thoroughly, and then drip it into an oil column filled with vacuum pump oil at 90 °C with a dispersing dropper to form it. Separate the formed gel balls from the oil and age them in an aging kettle at 140 °C for 10 hours. Wash the aged sol balls, then dry them at 60 °C for 12 hours to constant weight, and then calcine them at 650 °C for 5 hours to obtain alumina balls CSALO-2.
[0025] Comparative Example 3 Take 60 g of aluminum isopropoxide and 65 g of isopropanol and add them to a three-necked flask and place it in an 80 ℃ oil bath. Stir mechanically to dissolve the aluminum isopropoxide. Use a peristaltic pump to add 25 g of deionized water to the three-necked flask at a set flow rate of 20 g / h, keep the temperature at 80 ℃, and continue stirring for 30 minutes after the water is added. Transfer the above mixed slurry to a hydrothermal crystallization reactor and age at 120 ℃ for 4 h. The crystallized slurry is filtered and dried at 120 ℃ for 12 h until the product quality no longer changes, and the pseudo-boehmite sample CPB-3 is obtained.
[0026] The same method as in Example 1 was used to prepare alumina beads CSALO-3.
[0027] The specific surface area and pore volume of the alumina spheres of the present invention are measured by low temperature liquid nitrogen adsorption method. The physical properties of the alumina spheres are shown in Table 1.
[0028] Table 1 The experimental data showed that when the hydrolysis process of pseudo-boehmite was completed by using a rotating liquid film reactor, the specific surface area of the sample was further increased at a high shear rate. This was because the solid-liquid contact area was increased during the reaction, which promoted a large number of nuclei; EO 20 PO 10 EO 20 Compared with DMF as a template inducing agent, the prepared alumina spheres have larger pore volume and do not cause a decrease in specific surface area. It can be seen that the pseudo-boehmite prepared by combining the rotating liquid film reactor with the template-induced crystallization method has the characteristics of large specific surface area and large pore volume after oil column molding.
[0029] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing alumina spheres with large specific surface area and large pore volume, characterized in that: The following steps are involved: (a) adding aluminum alcoholate and an organic solvent to a rotating liquid film reactor at the same time, mixing, setting the temperature, and stirring to dissolve the aluminum alcoholate; (b) adding deionized water and a template inducing agent to the alcohol aluminum organic solution prepared in step (a), and stirring for a certain period of time to allow the solution to react fully; (c) transferring the mixed slurry of step (b) to a hydrothermal crystallization reactor for crystal growth, and setting a specific temperature and time for the crystallization reaction; (d) after the crystallization is completed, the material is discharged, filtered, and dried to a constant weight to obtain pseudo-boehmite powder; (e) dissolving the pseudo-boehmite obtained in step (d) in water to obtain a pseudo-boehmite suspension, and adding an acid solution for peptization; (f) adding a curing agent to the aluminum sol prepared in step (e); (g) dropping the slurry obtained in step (f) into a hot oil column to form spherical gel particles; (h) The gel beads obtained in step (g) are taken out and subjected to aging, washing, drying and calcination to obtain alumina beads.
2. The method according to claim 1, characterized in that The aluminum alcoholate in step (a) is one or more of aluminum methoxide, aluminum ethoxide, aluminum isopropoxide, aluminum sec-butoxide, aluminum n-hexoxide and aluminum isooctoxide; the organic solvent is one of isopropanol, n-butanol, sec-butanol, n-pentanol, n-hexanol and tetrahydrofuran; the molar ratio of the aluminum alcoholate to the organic solvent is 1:2-6; the dissolution temperature is 60-100°C, and the stirring speed is 300-600rpm.
3. The method according to claim 1, characterized in that In step (b), the molar ratio of the alcohol aluminum to the deionized water is 1:2-6; the stirring time is 10 min-2 h; the template inducing agent is EO 20 PO 10 EO 20 .
4. The method according to claim 1, characterized in that: In step (c), the crystallization temperature is 100-160° C. and the crystallization time is 4-14 h.
5. The method according to claim 1, characterized in that The drying temperature in step (d) is 80-120°C.
6. The method according to claim 1, characterized in that In step (e), the mass percentage of aluminum oxide in the pseudo-boehmite suspension is 5-30%; the mass ratio of the acid solution to the aluminum oxide in the pseudo-boehmite suspension is 0.1-1, and the pH is controlled at 2-5; the acid solution is one of the aqueous solutions of nitric acid, hydrochloric acid, sulfuric acid or formic acid with a mass percentage concentration of 3-30%.
7. The method according to claim 1, characterized in that In step (f), the mass ratio of the curing agent to the aluminum oxide in the aluminum sol is 0.2-0.6; the curing agent is hexamethylenetetramine, urea or a mixture of the two.
8. The method according to claim 1, characterized in that The molding oil in the hot oil column in step (g) is one of vacuum pump oil, machine oil, white oil, spindle oil, and mineral oil; and the temperature of the oil column is 90-99°C.
9. The method according to claim 1, characterized in that: In step (h), the aging temperature is 120-180°C, and the aging time is 12-48 h; the drying temperature is 50-100°C, and the drying time is 12-24 h; the roasting temperature is 550-1050°C, and the roasting time is 3-6 h.
Citation Information
Patent Citations
Pseudo-boehmite with large specific surface area and preparation method and application thereof
CN103172097A
Hydrothermally-stable spherical gamma-Al2O3 and preparation method thereof
CN104891538A
Exhaust gas disposable catalyst and method of manufacturing the same
US5242883A
Porous aluminum oxide materials prepared by non-ionic surfactant assembly route
US6027706A