V2O3-x (at) NC material and preparation method and application thereof

Through V2O3-x@NC material as the transduction layer, the problem of insufficient capacitance and interference of water layer in all-solid-state ion selective electrodes is solved, and high sensitivity and stable detection of chloride ions is achieved, with the detection limit reaching 10-5.45M. Ensure long-term stability of the electrode.

CN119038604APending Publication Date: 2024-11-29HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166666.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing all-solid ion selective electrodes have insufficient capacitance of the transducing layer material, resulting in insufficient signal conversion of chloride ion concentration, decreased detection sensitivity, and interference from the aqueous layer leads to unstable electrode potential.

Method used

V2O3-x@NC material is used as the transducing layer, and the alkyl amine intercalated vanadium pentoxide intermediate is formed by hydrothermal reaction between vanadium pentoxide and alkyl amine, and carbonize at high temperature to form a large pseudocapacitor and V2O3-x@NC composite material with excellent hydrophobic properties is used to construct all-solid chloride ion selective electrodes.

Benefits of technology

Fast and sensitive detection of chloride ions is achieved, the detection limit is improved to 10-5.45M, and the electrode stability is maintained during long-term use, avoiding the instability of the electrode potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038604A_ABST
    Figure CN119038604A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of ion analysis sensors, and discloses a V2O3-x (at) NC material and a preparation method and application thereof. The preparation method of the V2O3-x-coated NC material comprises the following steps: adding vanadium pentoxide into absolute ethyl alcohol, and stirring at room temperature to obtain dispersion liquid; alkylamine is added into the dispersion liquid for a hydrothermal reaction, and a product is obtained; and placing the dried product in a tubular furnace, heating to 600-700 DEG C in a nitrogen atmosphere, and then annealing for 2-3 hours to obtain V2O3-x (at) NC. The prepared V2O3-x (at) NC material is used as a transduction layer to modify the surface of a glassy carbon electrode to prepare the all-solid-state chloride ion selective electrode for chloride ion concentration detection. The method has good sensitivity, detection limit and excellent anti-interference capability, and has a good application prospect in the field of detection of chloride ions such as human sweat and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of ion analysis sensors, and more specifically relates to a V2O 3-x @NC materials, preparation methods and applications thereof. Background Art

[0002] Chloride ion is an important ion in body fluids. It is the main anion in the extracellular fluid of the human body. It plays an important role in regulating the acid-base balance, osmotic pressure and water distribution of the human body. Its content has important medical significance for the diagnosis of many diseases. Analysis of chloride ions in biological fluids can obtain rich information about personal health status and realize non-invasive detection of diseases. Due to the importance of chloride ion concentration detection, a reliable, accurate and rapid chloride ion detection method is very necessary.

[0003] Among the many detection methods for chloride ions, electrochemical detection is a very valuable method due to its convenience, rapidity and simple equipment. Potentiometric ion detection realized by ion-selective electrodes has recently become an important electrochemical detection method. The all-solid-state ion-selective electrode consists of an ion-selective membrane, a transduction layer and a conductive substrate. The transduction layer realizes the electrical signal conversion process from ions to electrons. However, the insufficient capacitance of the transduction layer material will cause the ion concentration signal to not be effectively converted into an electronic signal, resulting in a decrease in the detection sensitivity. At the same time, the formation of a water layer between the transduction layer and the conductive substrate will cause the potential to be greatly affected by interference, causing instability of the electrode potential during the measurement process. Therefore, it is very necessary to design and develop a large-capacitance and hydrophobic transduction layer to stabilize the electrode potential.

[0004] Vanadium-based materials are typical pseudocapacitive materials. Their rich oxidation states bring excellent capacitance and wide potential window, but their hydrophobicity is poor. Oxygen vacancies can narrow the band gap and improve the conductivity of vanadium-based materials. Combining vanadium-based materials with carbon is conducive to achieving the design goals of high capacitance and high hydrophobicity of the transduction layer, and realizing high-sensitivity and stable detection of chloride ions by all-solid-state chloride ion selective electrodes. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a V2O 3-x @NC material, its preparation method and application. This material, as the transduction layer material of the all-solid-state chloride ion selective electrode, can realize rapid and sensitive detection of chloride ions in solution and has higher stability.

[0006] The technical solution of the present invention is as follows:

[0007] V2O 3-x The preparation method of @NC material comprises the following steps:

[0008] (1) adding vanadium pentoxide to anhydrous ethanol and stirring at room temperature to obtain a dispersion;

[0009] (2) adding an alkylamine to the dispersion to carry out a hydrothermal reaction to obtain a product;

[0010] (3) The dried product is placed in a tube furnace, heated to 600-700°C in a nitrogen atmosphere, and then annealed for 2-3 hours to obtain V2O 3-x @NC.

[0011] Alkylamines include dodecylamine, hexadecylamine, octadecylamine and the like.

[0012] In a further embodiment, the concentration of the dispersion in step (1) is 0.025-0.1 mmol / ml.

[0013] In a further embodiment, the molar ratio of vanadium pentoxide to alkylamine in step (2) is 1:1;

[0014] The hydrothermal reaction is carried out at 70-80° C. with continuous stirring for 36-48 hours.

[0015] The second invention object of the present invention is to provide V2O prepared by the above preparation method. 3-x @NC Materials.

[0016] The third invention object of the present invention is to provide the above-mentioned V2O 3-x @Application of NC materials, which are used as transduction layer materials in all-solid-state chloride ion selective electrodes.

[0017] In a further embodiment, the method for preparing the all-solid-state chloride ion selective electrode comprises the following steps:

[0018] (1) V2O 3-x @NC material is ultrasonically dispersed in deionized water to form a dispersion with a concentration of 5-30 mg / ml;

[0019] (2) dripping the dispersion onto the surface of the glassy carbon electrode, and forming a transduction layer on the surface of the glassy carbon electrode after drying;

[0020] (3) Then, a chloride ion selective membrane solution is drop-coated on the surface of the transfer layer and dried to obtain a fully solid-state chloride ion selective electrode.

[0021] In a further embodiment, the all-solid-state chloride ion selective electrode is first stored at 10 -3 NaCl solution for at least 12 h, then transferred to 10 -9 Activate with NaCl solution for 8-10h.

[0022] In a further embodiment, the detection limit of the all-solid-state chloride ion selective electrode for chloride ions is 10 -5.45M.

[0023] In a further embodiment, the all-solid-state chloride ion selective electrode is used to detect chloride ions in a solution or human sweat.

[0024] The advantages of the present invention are:

[0025] 1. The present invention hydrothermally reacts vanadium pentoxide with alkylamine to form an alkylamine intercalated vanadium pentoxide intermediate, forming a lamellar structure. Since the intercalation and exfoliation of the alkyl chain increases the specific surface area of ​​the oxide and the formation of the carbon layer, it has excellent hydrophobic properties and the maximum contact angle can reach 138.4°.

[0026] 2. Then, the alkylamine intercalated vanadium pentoxide intermediate is carbonized. At high temperature, the vanadium pentoxide undergoes a redox reaction, resulting in the removal of some oxygen atoms to form vanadium trioxide with oxygen defects (V2O 3-x At the same time, the alkylamine undergoes pyrolysis to form nitrogen-doped carbon (NC), which also reacts with oxygen-deficient vanadium trioxide (V2O 3-x ) to generate V2O 3-x @NC composites. So V2O 3-x @NC materials have unique electrical, magnetic and mechanical properties.

[0027] 3. V2O prepared by the present invention 3-x @NC material has large pseudocapacitance and excellent hydrophobic properties, so using this material as a transduction layer to construct an all-solid-state chloride ion selective electrode has great application prospects and commercial value.

[0028] 4. The present invention uses V2O 3-x The all-solid-state chloride ion selective electrode constructed with @NC as the transduction layer has good selectivity for chloride ion detection and low detection limit. -5 -10 -1 The linear range of M showed a near-Nernstian response of 58.23 mV / dec to chloride ions, and the detection limit of chloride ions reached 10 -5.45 M. At the same time, due to the excellent hydrophobicity of the transduction layer material, the chloride ion selective electrode does not contain an interfacial water layer between the transduction layer and the conductive substrate, has excellent stability, and can be used without repeated calibration in long-term use. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the scanning electron microscope image of Experimental Example 1.

[0030] Figure 2 is the X-ray diffraction spectrum of Experimental Example 2,

[0031] Figure 3 V2O 3-x @NC and V2O3-x Contact angle comparison chart,

[0032] Figure 4 V2O 3-x @NC and V2O 3-x Comparison of electron paramagnetic resonance spectra,

[0033] Figure 5 V2O 3-x @NC cyclic voltammetry curves of different mass loadings,

[0034] Figure 6 V2O 3-x @NC, V2O 3-x Short-term stability measured for the transduction layer and coated silk all-solid-state chloride ion selective electrodes,

[0035] Figure 7 V2O 3-x @NC, V2O 3-x Impedance and water layer tests for transduction layer and coated silk all-solid-state chloride ion selective electrodes,

[0036] Figure 8 V2O 3-x @NC, V2O 3-x Potential response graphs and calibration curves measured for the transduction layer and coated silk all-solid-state chloride ion selective electrodes. DETAILED DESCRIPTION

[0037] The present invention will be further explained below in conjunction with the embodiments and drawings, but the present invention is not limited thereto.

[0038] The reagents and materials used in the following examples are all commercially available products, and all reagents can be used directly without further purification.

[0039] Example 1: V2O 3-x Preparation of @NC:

[0040] 1mM vanadium pentoxide was added to 15mL anhydrous ethanol and magnetically stirred at room temperature for 30 minutes to obtain a brown-yellow turbid solution; then 1mM hexadecylamine was added and stirred continuously at 80°C for 48h for hydrothermal reaction. After the product cooled to room temperature, it was washed with anhydrous ethanol and ultrapure water three times respectively, and then the product was transferred to 60°C for vacuum drying for 24h. The dried powder was placed in a tube furnace and annealed at 650°C for two hours in a nitrogen atmosphere to obtain V2O 3-x @NC Materials.

[0041] Test Example 1:

[0042] The raw material vanadium pentoxide and the hexadecylamine intercalated vanadium pentoxide intermediate prepared in Example 1 and V2O 3-x@NC materials were observed under a scanning electron microscope. The scanning electron microscope images are shown in Figure 1 As shown, Figure 1 A is a scanning electron microscope image of vanadium pentoxide, and B is a scanning electron microscope image of a hexadecylamine intercalated vanadium pentoxide intermediate. The hexadecylamine inserted in situ by the hydrothermal method exfoliates the bulk vanadium pentoxide to form a lamellar structure. Figure 1 C in the formula is V2O 3-x @NC, hexadecylamine was in situ converted into carbon layers, forming the wrinkled morphology.

[0043] Test Example 2:

[0044] The raw material vanadium pentoxide and the hexadecylamine intercalated vanadium pentoxide intermediate prepared in Example 1 and V2O 3-x @NC materials were analyzed by X-ray powder diffractometer, and their X-ray diffraction spectra are shown in Figure 2 shown.

[0045] Depend on Figure 2 It can be seen that after the insertion of hexadecylamine, its phase remains unchanged, which is V2O5 (same as the XRD standard spectrum card PDF 41-1426 of V2O5), and a new diffraction peak appears at a low angle of 6.22°, indicating that the alkylamine has been successfully inserted into the middle layer of vanadium pentoxide; according to the Bragg diffraction formula, the interlayer spacing is calculated to be The final phase after carbonization is V2O3 (same as the XRD standard spectrum card of V2O3 PDF 34-0187). This shows that Example 1 of the present application successfully prepared V2O3. 3-x @NC Materials.

[0046] Comparative Example 1:

[0047] The vanadium pentoxide was annealed at 600°C for 6 h in a 5% (volume ratio) hydrogen-argon mixed gas to obtain an oxygen-deficient vanadium trioxide material (V2O 3-x ).

[0048] Test Example 3:

[0049] The V2O prepared in Example 1 3-x @NC and V2O prepared in Comparative Example 1 3-x The contact angle is measured, such as Figure 3 As shown, V2O 3-x The contact angle of @NC is much larger than that of V2O 3-x , indicating that it has excellent hydrophobic properties, which is beneficial to resist the formation of water layer when used as a transduction layer.

[0050] Test Example 4: V2O 3-x @NC and V2O 3-x Comparison of electron paramagnetic resonance spectra

[0051] like Figure 4 As shown, the signal at g = 2.004 belongs to the oxygen vacancy. 3-x The oxygen vacancy signal in NC is higher than that in V2O 3-x , indicating that it has a higher oxygen vacancy concentration, which is due to the activation of the active volume by the exfoliation caused by the insertion of alkylamine during its preparation process.

[0052] Embodiment 2:

[0053] 1mM vanadium pentoxide was added to 20mL anhydrous ethanol and magnetically stirred at room temperature for 30 minutes to obtain a brown-yellow turbid solution; then 1mM dodecylamine was added and stirred continuously at 70°C for 40h for hydrothermal reaction. After the product cooled to room temperature, it was washed with anhydrous ethanol and ultrapure water three times respectively, and then the product was transferred to 60°C for vacuum drying for 24h. The dried powder was placed in a tube furnace and heated to 600°C in a nitrogen atmosphere for annealing for 2.5 hours to obtain V2O 3-x @NC Materials.

[0054] Embodiment 3:

[0055] 1mM vanadium pentoxide was added to 40mL anhydrous ethanol and magnetically stirred at room temperature for 30 minutes to obtain a brown-yellow turbid solution; then 1mM octadecylamine was added and stirred continuously at 75°C for 36 hours for hydrothermal reaction. After the product cooled to room temperature, it was washed with anhydrous ethanol and ultrapure water three times respectively, and then the product was transferred to 60°C for vacuum drying for 24 hours. The dried powder was placed in a tube furnace and heated to 700°C in a nitrogen atmosphere for annealing for 3 hours to obtain V2O 3-x @NC Materials.

[0056] Example 4: Preparation of all-solid-state chloride ion selective electrode:

[0057] (1) Preparation of chloride ion selective polymer membrane

[0058] The chloride ion selective membrane mixture is composed of 2.0wt% chloride ion carrier III (3,6-docosanyloxy-4,5-dimethyl-o-phenylene-bis(mercuric chloride)), 1.2wt% tridodecylmethylammonium chloride (anion exchanger), 33.0wt% polyvinyl chloride and 63.8wt% dioctyl sebacate. A total of 0.2g of the mixture is dissolved in 2mL of tetrahydrofuran, stirred at room temperature for three hours to form a uniform solution, and stored in a desiccator for later use.

[0059] (2) Grind the glassy carbon electrode, clean it ultrasonically, and then blow dry it under nitrogen for later use;

[0060] (3) The V2O prepared in Example 1 3-x@NC materials were ultrasonically dispersed in deionized water to form dispersions with concentrations of 5, 10, 15, 20, 25, and 30 mg / ml;

[0061] (4) 10 μL of the above dispersions of each concentration were dripped onto the surface of the glassy carbon electrode as the transduction layer, with the loading amounts being 0.05, 0.10, 0.15, 0.20, 0.25 and 0.30 mg, respectively, and dried under natural conditions for 12 hours;

[0062] (5) Then, 80 μL of chloride ion selective membrane solution was drop-coated on the surface and dried to obtain a solid-state chloride ion selective electrode (GC / V2O 3-x @NC / Cl - -ISM).

[0063] Comparative Example 2:

[0064] Preparation of GC / V2O in the same manner as in Example 4 3-x / Cl - -ISM, the only difference is that the transfer layer material is the vanadium trioxide material of Comparative Example 1.

[0065] Comparative Example 3:

[0066] Preparation of coated silk GC / Cl in the same manner as in Example 4 - -ISM, the only difference is that no transduction layer material is dripped on the surface of the glassy carbon electrode.

[0067] Experimental Example 5: V2O supported on glassy carbon electrode 3-x @NC drip amount selection

[0068] Based on the loaded V2O obtained in step (4) of Example 4 3-x @NC glassy carbon electrode, the drop volume of the transfer layer material was optimized by electrochemical cyclic voltammetry, specifically: the electrode was placed at 10 -1 Cyclic voltammetry was performed using a three-electrode system in a 1.4 M NaCl electrolyte solution. The parameters were as follows: potential window -0.5 to 0.5 V, scan rate 100 mV s -1 . Get Figure 5 The cyclic voltammetry curve is shown.

[0069] Depend on Figure 5 As can be seen in A and B, the added mass load is 0.20 mg of V2O 3-x The glassy carbon electrode of @NC has a larger current response, indicating that its optimal loading volume is 0.20 mg.

[0070] Test Example 6: Stability test of all-solid-state chloride ion selective electrode

[0071] Based on the V2O3-x @NC's all-solid-state chloride ion selective electrode (GC / V2O 3-x @NC / Cl - -ISM, and its short-term stability was characterized by chronopotentiometry and compared with that based on vanadium trioxide (GC / V2O 3-x / Cl - -ISM) and the coated silk in Comparative Example 3 (GC / Cl - -ISM) all-solid-state chloride ion selective electrodes. Specifically, before the test, each all-solid-state chloride ion selective electrode was heated to 10 -3 The activated electrode was then placed in a 10 -1 The three-electrode system was used to perform the chronopotentiometry test in a 100 M sodium chloride solution. The parameters are as follows: applied current: +1 nA and -1 nA, each for 60 s. Figure 6 The chronopotential comparison diagram is shown.

[0072] Depend on Figure 6 It can be seen that the transduction layer V2O 3-x The introduction of @NC significantly reduced the potential drift of the all-solid-state ion-selective electrode and significantly improved the stability of the electrode.

[0073] Experimental Example 7: Electrochemical impedance spectroscopy and water layer test of all-solid-state chloride ion selective electrode Based on the V2O 3-x @NC's all-solid-state chloride ion selective electrode (GC / V2O 3-x @NC / Cl - -ISM) was used to characterize its ion-electron transduction properties by electrochemical impedance spectroscopy and compared with that based on VO 3-x (GC / V2O 3-x / Cl - -ISM) and coated wire (GC / Cl - -ISM) chloride ion selective electrodes were used for performance comparison.

[0074] Specifically: the activated electrode is heated for 10 -1 M sodium chloride solution, using a three-electrode system for electrochemical impedance spectroscopy. The parameters are as follows: Frequency range: 0.01-10 5 Hz, with an amplitude of 100mV. Figure 7 Electrochemical impedance comparison diagram shown.

[0075] Depend on Figure 7 It can be seen that compared with the electrode without the transduction layer material, the introduction of the transduction layer reduces the contact impedance (the contact impedance between the interface of the membrane and the conductive substrate) and increases the diffusion rate of ions and electrons between the interfaces.

[0076] In the water layer test, based on the V2O 3-x The all-solid-state chloride ion selective electrode of @NC exhibits a stable potential response and is not affected by interfering ions, indicating that the transduction layer has excellent hydrophobicity and can resist the formation of a water layer.

[0077] Test Example 8: Application of all-solid-state chloride ion selective electrode in chlorine detection

[0078] Based on the V2O 3-x @NC's all-solid-state ion selective electrode, the activated electrode (all-solid-state chloride ion selective electrode at 10 -3 M sodium chloride aqueous solution for 12 h, and then -9 The chloride ions in the solution were detected by activating the solution in a sodium chloride aqueous solution of 50 M for 9 h.

[0079] Specifically, the open circuit potential of the electrode was tested using an electrochemical workstation, using a two-electrode system, with Ag / AgCl as the reference electrode connected to a 1M lithium acetate salt bridge, and the prepared all-solid-state chloride ion selective electrode as the working electrode. The open circuit potential of the electrode was tested in chloride ion solutions of different concentrations under the background of ultrapure water, and the corresponding potential-time curve and calibration (logarithm of activity vs. potential) curve were plotted, see Figure 8 .

[0080] Firstly, the all-solid-state chloride ion selective electrode was measured at 10 -1 M, 10 -2 M, 10 -3 M, 10 -4 M, 10 -5 M, 10 -6 M and 10 -7 M chloride ion concentration, and record its potential-time curve (such as Figure 8 Then, the concentration of the sodium chloride aqueous solution with different concentrations is corrected to the activity, and then the calibration curve is drawn. Figure 8 The calibration curve of B shows that GC / V2O 3-x @NC / Cl - -ISM in NaCl concentration of 10 -1 -10 -5 mol L -1 The aqueous solution showed a Nernst response with a response slope of 58.23 mV / dec and a detection limit of 10 -5.45 M. The results show that based on V2O 3-x @NC's all-solid-state ion-selective electrode has better sensitivity and lower detection limit, and the detection limit of this electrode meets the requirements for the detection of chloride ions in sweat.

[0081] Test Example 9: V2O in human sweat 3-x @NC testing and verification

[0082] The V2O based 3-x @NC's all-solid-state ion-selective electrode is used to detect chloride ions in human sweat.

[0083] Specifically, the constructed all-solid-state chloride ion selective electrode is used as an indicator electrode and the Ag / AgCl reference electrode is connected to a 1M lithium acetate salt bridge, and the concentration of chloride ions in artificial sweat is tested using the standard addition method, and compared with the test results of ion chromatography (HPIC). The results show that the test results of the chloride ion selective electrode constructed by the present invention are consistent with the test results of HPIC.

[0084] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those familiar with the art can easily make various modifications to the implementation cases and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the implementation cases here, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. V 2 O 3-x @NC material preparation method, Features: The following steps are involved: (1) adding vanadium pentoxide to anhydrous ethanol and stirring at room temperature to obtain a dispersion; (2) adding an alkylamine to the dispersion to carry out a hydrothermal reaction to obtain a product; (3) The dried product is placed in a tube furnace, heated to 600-700°C in a nitrogen atmosphere, and then annealed for 2-3 hours to obtain V 2 O 3-x @NC.

2. The preparation method according to claim 1, Features: The concentration of the dispersion in step (1) is 0.025-0.1 mmol / ml.

3. The preparation method according to claim 1, Features: In step (2), the molar ratio of vanadium pentoxide to alkylamine is 1:1; The alkylamine includes dodecylamine, hexadecylamine or octadecylamine; The hydrothermal reaction is carried out at 70-80° C. with continuous stirring for 36-48 hours.

4. V prepared by the preparation method according to any one of claims 1 to 3 2 O 3-x @NC Materials.

5. V according to claim 4 2 O 3-x @Application of NC materials, Features: It is used as the transduction layer material in the all-solid-state chloride ion selective electrode.

6. The use according to claim 5, Features: The preparation method of the all-solid-state chloride ion selective electrode comprises the following steps: (1) V 2 O 3-x @NC material is ultrasonically dispersed in deionized water to form a dispersion with a concentration of 5-30 mg / ml; (2) dripping the dispersion onto the surface of the glassy carbon electrode, and forming a transduction layer on the surface of the glassy carbon electrode after drying; (3) Then, a chloride ion selective membrane solution is drop-coated on the surface of the transfer layer and dried to obtain a fully solid-state chloride ion selective electrode.

7. The use according to claim 5, Features: The all-solid-state chloride ion selective electrode was stored at 10 -3 NaCl solution for at least 12 h, then transferred to 10 -9 Activate with NaCl solution for 8-10h.

8. The use according to claim 5, Features: The detection limit of the all-solid-state chloride ion selective electrode for chloride ions is 10 -5.45 M.

9. The use according to claim 5, Features: The all-solid-state chloride ion selective electrode is used for detecting chloride ions in a solution or human sweat.