Fe8O8 (OH) 8Cl1.35 catalyst as well as preparation method and application thereof

The preparation of Fe8O8(OH)8Cl1.35 catalyst is solved by a one-step solid-phase sintering method, which solves the problems of complex traditional methods and insufficient research on iron-based semiconductor photocatalysts, and achieves high-efficiency photohydrolysis and environmentally friendly photocatalytic properties, which are suitable for industrial applications.

CN119038618AActive Publication Date: 2024-11-29CARBON TRANSFER (TANGSHAN) TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411529969.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-29
Estimated Expiration
2044-10-30

AI Technical Summary

Technical Problem

Traditional oxide semiconductor photocatalytic materials have problems such as limited light absorption range, high electron-hole recombination rate, poor light stability, limited selectivity, and low carrier mobility in the photocatalytic field, and research on iron-based semiconductor photocatalysts Fewer, the preparation method is complex and difficult to achieve industrial application.

Method used

A simple one-step solid phase sintering method is used to prepare Fe8O8(OH)8Cl1.35 catalyst. By grinding the raw material of ferric chloride hexahydrate, sintering it in the heating device, controlling the heating rate and temperature, avoiding the use of organic additives and acids Base regulation to obtain a catalyst with rod-like cluster structure composed of nanoparticles.

Benefits of technology

It realizes efficient photolysis of aquatic hydrogen performance, improves the stability and light stability of the catalyst, reduces production costs and energy consumption, simplifies the process flow, is suitable for large-scale production, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038618A_ABST
    Figure CN119038618A_ABST
Patent Text Reader

Abstract

The invention belongs to but not limited to the technical field of photocatalytic materials, and discloses a Fe8O8 (OH) 8Cl < 1.35 > catalyst and a preparation method and application thereof.The Fe8O8 (OH) 8Cl < 1.35 > catalyst is prepared with ferric chloride hexahydrate as a raw material through a low-temperature calcination method, the microstructure of the prepared Fe8O8 (OH) 8Cl < 1.35 > nanomaterial is a cluster structure composed of nanorods, the particle size of rod clusters is about 100-1000 nm, and the particle size of the rod clusters is about 10-20 nm. And the surface contains abundant unsaturated bonds as adsorption sites. Different from a traditional preparation method adopting a hydrothermal method and adding an active agent for regulation and control, a solid-phase reaction preparation method is adopted, and the synthesis method of the Fe8O8 (OH) 8Cl1.35 rodlike nano material is enriched. The Fe < 8 > O < 8 > (OH) < 8 > Cl < 1.35 > nano material prepared by the method disclosed by the invention shows obvious photocatalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photocatalytic materials but is not limited to it, and particularly relates to a Fe8O8(OH)8Cl 1.35 Catalyst, preparation method and use thereof. Background Art

[0002] In recent years, environmental pollution and resource shortages have become increasingly serious, posing a serious threat to the sustainable development of human society. Photocatalytic technology can use sunlight to drive chemical reactions, decompose water to produce clean energy hydrogen, reduce carbon dioxide to high-efficiency chemical fuels, or degrade pollutants in industrial and domestic wastewater, thereby helping to solve the energy crisis and alleviate environmental degradation. The core of semiconductor photocatalytic technology is the targeted development of semiconductor materials, that is, photocatalysts. Most traditional oxide semiconductor photocatalytic materials have limited light absorption range, high electron-hole recombination rate, poor photostability, limited selectivity, and low carrier mobility. These shortcomings have prompted researchers to continuously explore and develop new semiconductor photocatalyst materials. Among various new photocatalysts, the research on iron-based semiconductor photocatalysts is relatively small. This is because the application research of iron-based semiconductor materials in the field of photocatalysis started late, and there are some challenges in the photocatalytic performance of iron-based semiconductor materials, such as stability and visible light absorption capacity. Although some literatures involve the research progress of various composite semiconductor photocatalysts and iron-based metal organic framework materials such as titanium-based, zinc-based, and tungsten-based composite ferrites, research specifically on iron-based semiconductor photocatalysts is rarely mentioned. This shows that the research and application of iron-based semiconductor photocatalysts in the field of photocatalysis need to be further developed and explored. With the increasing demand for new photocatalysts, iron-based semiconductor photocatalysts will become an important direction for future research. 1.35 Nanomaterials are a good semiconductor photocatalyst material, but research on this material is extremely rare, and the only synthesis method is the traditional hydrothermal method, and most of them are prepared with organic active agents. This method is difficult to achieve industrial application due to its high equipment requirements, long reaction time, low product purity, organic by-products, and difficulty in large-scale production. Therefore, there is a need for a Fe8O8(OH)8Cl 1.35 A method for preparing a catalyst. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention provides a Fe8O8(OH)8Cl 1.35 Catalyst, preparation method and use thereof.

[0004] The present invention is achieved by: a Fe8O8(OH)8Cl 1.35The catalyst is prepared by a simple one-step solid phase sintering method, comprising the following steps: (1) Grind the ferric chloride hexahydrate raw material.

[0005] (2) The ground ferric chloride hexahydrate powder with uniform particles is placed in a container, and then the ferric chloride hexahydrate powder is placed in a heating device, and a temperature rising program is set to perform sintering.

[0006] (3) The temperature is lowered to room temperature, the sludge product obtained by sintering is cleaned, and the cleaned product is dried to obtain Fe8O8(OH)8Cl 1.35 catalyst.

[0007] Furthermore, in step (1), the ferric chloride hexahydrate raw material needs to be ground in a dry environment to prevent hydrolysis of the raw material.

[0008] Furthermore, in step (2), the amount of raw materials loaded in the container should be no less than half of its capacity, otherwise other by-products are likely to be generated. For example, it can be 2 / 3 of the container volume.

[0009] Furthermore, in step (2), the container should be covered with a lid after the raw materials are loaded to prevent the product from volatilizing.

[0010] Furthermore, in step (2), the programmed heating rate is 10°C / min, and the calcination temperature is maintained at 160-280°C, for example, 200°C.

[0011] According to the present invention, in step (4), the muddy product is brown and contains a variety of soluble impurities, and needs to be washed with water. As an illustrative example, it is ultrasonically cleaned with deionized water for 3 times, and then dried and collected after centrifugation.

[0012] Furthermore, the sample loading volume should be greater than half of the container volume.

[0013] Furthermore, in step (2), the sintering working atmosphere is air.

[0014] Furthermore, in step (3), the calcination temperature is 160-280°C.

[0015] Another object of the present invention is to provide a Fe8O8(OH)8Cl 1.35 Catalyst preparation method Fe8O8(OH)8Cl prepared 1.35 The catalyst has a microstructure of a rod-like cluster structure composed of nanoparticles, and the average particle size of a single nanorod is about 5-300nm.

[0016] Preferably, the average particle size is 50-100 nm, and more preferably, the average particle size is 100 nm.

[0017] During the preparation process, it is prepared by a simple one-step calcination method and is carried out at a low temperature without applying a high temperature.

[0018] Another object of the present invention is to provide a Fe8O8(OH)8Cl 1.35 Catalyst used for photocatalytic hydrogen production. Fe8O8(OH)8Cl 1.35 The photocatalyst can produce hydrogen at a rate of 2.05 μmol g -1 h -1 .

[0019] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows: First, due to Fe8O8(OH)8Cl 1.35 The material is not easy to synthesize stably and occasionally appears as an intermediate product of chemical synthesis. Related research is relatively rare, and the hydrothermal synthesis method used in the rare literature requires the addition of organic additives and the regulation of pH to promote the stable synthesis of the material. The present invention provides a new method for preparing Fe8O8(OH)8Cl 1.35 The method of material, that is, a one-step calcination method, directly calcining the raw materials in a muffle furnace to prepare stable Fe8O8(OH)8Cl 1.35 The preparation method has low raw material price, simple operation, safety, high yield, easy stable synthesis and large-scale production. The technical method provided by the present invention solves the problem that the material is not easy to be synthesized stably, and compared with the traditional synthesis route, there is no need to use organic additives and pH control, less harmful waste liquid is generated during the preparation process, and it is more friendly to the ecological environment.

[0020] Fe8O8(OH)8Cl of the present invention 1.35 Nanomaterials can be used as photocatalyst materials and have good photostability.

[0021] Second, Fe8O8(OH)8Cl 1.35 The material can use solar energy to decompose water to produce hydrogen, and can also degrade organic pollutants, which is of great significance to environmental protection; Fe8O8(OH)8Cl 1.35 The material exhibits good activity in the photocatalytic process and is expected to improve the conversion efficiency of solar energy to chemical energy, which has potential value for the development of sustainable energy technology; cost-effectiveness, the catalyst raw materials involved in the present invention are easy to obtain, low-cost, can be mass-produced and maintain their photocatalytic performance, it is more cost-effective than some existing photocatalysts, thereby reducing the economic threshold of clean energy and sewage treatment; nanomaterials usually have unique physical and chemical properties, Fe8O8(OH)8Cl 1.35The research and application of nanocatalysts will promote technological progress in related fields, create new scientific research results and patents, and increase their commercial value. 1.35 The expected benefits and commercial value of materials as photocatalysts lie in their potential applications in environmental protection, energy conversion, cost-effectiveness and technological innovation. Of course, the specific economic benefits also need to consider the actual production costs, market acceptance and feasibility of large-scale applications.

[0022] The technical solution of the present invention fills the technical gap in the industry at home and abroad: At present, about Fe8O8(OH)8Cl 1.35 The research on the material is still relatively rare, and its synthesis method, structural characteristics, potential applications, etc. need to be studied and developed urgently. The technical solution provided by the present invention adopts a simple one-step solid phase calcination method to directly calcine the raw materials at a suitable temperature, and completes the preparation of Fe8O8(OH)8Cl in one step without acid and alkali regulation and template additive conditions. 1.35 Catalyst. The technical method fills Fe8O8(OH)8Cl 1.35 There are gaps in areas related to material synthesis methods and solar energy conversion applications.

[0023] The technical solution of the present invention solves the technical problems that people have been eager to solve but have never been successful: the one-step calcination method avoids the multiple heat treatments and intermediate product separation steps in the traditional synthesis method, shortens the entire production cycle, and due to the omission of complex post-processing steps, the conversion rate of raw materials to target products is higher, which helps to improve the overall yield; simplifying the process can reduce energy consumption, which is particularly important for large-scale industrial production. The simplicity and ease of operation of the one-step calcination method makes it easier to scale up the process to industrial production scale, which is conducive to reducing the manufacturing cost of unit products; by accurately controlling the calcination temperature and time, the microstructure and physical and chemical properties of the final product can be better regulated to ensure the consistency of product quality. The technical solution of the present invention can simplify the production process, improve yield, save energy and reduce consumption, scale production, and improve quality controllability.

[0024] Third, the technical solution of the present invention solves many problems in the prior art in industrial applications and brings about significant technological progress, which is specifically manifested as follows: 1. The complexity of the preparation process.

[0025] Problems with existing technologies: Traditional processes for preparing similar catalysts are often complicated, usually requiring multi-step chemical reactions or high-temperature treatments, involving tedious solvent preparation and treatment, which increases time costs and process difficulty. In addition, these methods have a significant impact on the environment and high waste disposal costs.

[0026] Technological progress: The present invention adopts a one-step solid-phase sintering method, avoiding cumbersome liquid-phase reactions or multi-step chemical treatments. Through simple grinding, sintering and cleaning steps, efficient catalysts can be quickly obtained, greatly reducing process complexity and production costs. This process not only simplifies the process, but is also more environmentally friendly, reducing the use of solvents and waste emissions, and improving the sustainability of the process.

[0027] 2. The problem of unstable or uneven catalyst performance.

[0028] Problems with existing technologies: Many traditional catalysts are prone to unstable performance and uneven activity during the preparation process, which affects their application in actual industrial reactions. Especially in multiphase reactions, the activity of the catalyst will be affected by the surface morphology and structural heterogeneity.

[0029] Technological progress: The present invention ensures the Fe8O8(OH)8Cl by precisely controlling the grinding and sintering temperature of ferric chloride hexahydrate. 1.35 The structural uniformity and stability of the catalyst. The grinding process increases the specific surface area of ​​the material. The oxide and chloride structures formed during the sintering process are tightly combined, producing more stable catalytic active sites, ensuring the stability and uniformity of the catalyst under different reaction conditions. This technical improvement greatly improves the performance consistency of the catalyst and enhances the reliability of industrial applications.

[0030] 3. The problem of high production costs.

[0031] Existing technical problems: Traditional catalyst preparation processes usually involve high-temperature multi-step treatments, high equipment requirements, harsh reaction conditions, and long production times, resulting in high production costs and difficulty meeting the needs of large-scale industrial applications.

[0032] Technological progress: The solid phase sintering method of the present invention does not require complex equipment and high-cost raw materials. The catalyst can be efficiently produced through a simple high-temperature sintering process. The method reduces the consumption of raw materials and energy, and the process equipment requirements are relatively simple, making the scale of catalyst production possible and reducing the production cost in large-scale applications. The process is economical and efficient, and is suitable for industrial promotion, especially mass production in the field of catalysts.

[0033] 4. The problem of insufficient catalytic efficiency and environmental performance.

[0034] Problems with existing technologies: Traditional catalysts show certain catalytic efficiency in multiphase reactions, but their activity tends to decay as the reaction time increases. At the same time, harmful by-products are produced during the preparation of these catalysts, which is not environmentally friendly.

[0035] Technological progress: Fe8O8(OH)8Cl prepared by the present invention 1.35The catalyst not only exhibits high catalytic activity in multiphase reactions, but also has good structural stability and long-term catalytic ability, and can maintain high catalytic efficiency for a long time. In addition, this method does not involve the use of harmful chemicals, and by-products are removed by washing, making the entire process clean and environmentally friendly. This environmentally friendly production method further enhances the application value of the catalyst and meets the current industry's demand for green manufacturing.

[0036] The present invention solves the problems of complicated process, unstable catalyst performance, high production cost and insufficient environmental performance in the prior art through a simple one-step solid phase sintering method. Its significant technical progress is reflected in the simplification of process, improvement of catalyst performance, reduction of production cost and environmental friendliness. It has a wide range of industrial application prospects and is particularly suitable for large-scale production and application in the field of catalysis.

[0037] Fourth, the parameter setting and process optimization of the present invention solve multiple problems in the prior art in industrial applications and have achieved significant technological progress, which is specifically reflected in the following aspects: 1. Technical problems solved.

[0038] (1) Low catalyst purity leads to unstable performance.

[0039] In the prior art, since impurities are difficult to remove effectively during the preparation process, the purity and performance of the catalyst are unstable, which directly affects the use effect of the catalyst. In particular, the accumulation of impurities in multiple catalytic reactions will accelerate the deactivation of the catalyst.

[0040] (2) The sintering process is not precisely controlled and the crystal phase stability is poor.

[0041] In traditional catalyst preparation processes, the sintering temperature and heating rate are difficult to accurately control, resulting in an unstable crystal structure, which in turn affects the catalytic activity and durability of the catalyst.

[0042] (3) Raw material hydrolysis problem.

[0043] Raw materials such as ferric chloride hexahydrate are prone to hydrolysis in a humid environment, which causes changes in the raw material structure and affects the composition and performance of the catalyst. The existing technology lacks environmental control for grinding and raw material processing, and the hydrolysis problem has a negative impact on the process.

[0044] 2. Significant technological progress.

[0045] (1) High-precision measurement and control improve catalyst purity and stability.

[0046] The present invention effectively solves the problem of low catalyst purity by optimizing the catalyst preparation process, especially the precise setting of the cleaning and drying steps. Specifically, in step (3), impurities are completely removed by ultrasonic cleaning with deionized water and repeated centrifugation operations, so that the final Fe8O8(OH)8Cl 1.35 The catalyst has higher purity and more stable catalytic performance.

[0047] (2) Precise heating rate and sintering temperature control ensures crystal phase stability.

[0048] The present invention significantly improves the stability of the crystal phase by precisely controlling the heating rate (10°C / min) and calcination temperature (160-280°C) during the sintering process. This precise temperature control design avoids over-sintering or under-sintering and ensures the stability of Fe8O8(OH)8Cl 1.35 The structural integrity of the catalyst significantly improves its catalytic activity and service life.

[0049] (3) Hydrolysis control solves the problem of raw material stability.

[0050] In order to solve the problem of hydrolysis of raw materials during the preparation process, the present invention introduces a process flow of grinding ferric chloride hexahydrate in a dry environment in step (1), thereby avoiding hydrolysis of the raw materials in a humid environment. Through this control, the chemical properties of the raw materials are fully protected, ensuring that Fe8O8(OH)8Cl 1.35 The stability of the catalyst components, thereby improving its final performance.

[0051] 3. Impact of industrial applications.

[0052] The present invention significantly improves the Fe8O8(OH)8Cl 1.35 The purity, crystal phase stability and catalytic performance of the catalyst make its application in industrial catalytic reactions more competitive. Its precise temperature control and material processing process not only improves the quality of the product, but also reduces the production cost and enhances the market competitiveness of the product. Especially in the fields of environmental catalysis, waste gas treatment and chemical catalysis, the present invention can significantly improve the reaction efficiency, reduce the problem of catalyst deactivation, and provide an efficient and reliable technical solution for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 It is Fe8O8(OH)8Cl provided in Examples 1-4 of the present invention. 1.35 Flow chart of the catalyst preparation method.

[0054] Figure 2 It is Fe8O8(OH)8Cl provided in Example 3 of the present invention. 1.35Schematic diagram of the catalyst structure.

[0055] Figure 3 It is Fe8O8(OH)8Cl provided in Example 3 of the present invention. 1.35 X-ray diffraction pattern of catalyst.

[0056] Figure 4 It is Fe8O8(OH)8Cl provided in Example 3 of the present invention. 1.35 UV-visible absorption spectrum of the catalyst.

[0057] Figure 5 It is Fe8O8(OH)8Cl provided in Examples 1-4 of the present invention. 1.35 Photocatalytic hydrogen production performance diagram of the catalyst. DETAILED DESCRIPTION

[0058] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0059] like Figure 1 As shown, a Fe8O8(OH)8Cl 1.35 The catalyst is prepared by a simple one-step solid phase sintering method, comprising the following steps: (1) Grind the ferric chloride hexahydrate raw material.

[0060] (2) The ground ferric chloride hexahydrate powder with uniform particles is placed in a container, and then the ferric chloride hexahydrate powder is placed in a heating device, and a temperature rising program is set to perform sintering.

[0061] (3) The temperature is lowered to room temperature, the sludge product obtained by sintering is cleaned, and the cleaned product is dried to obtain Fe8O8(OH)8Cl 1.35 catalyst.

[0062] Fe8O8(OH)8Cl of the present invention 1.35 The catalyst preparation method adopts a one-step solid-phase sintering method, which is simple and efficient. The specific working principle is as follows: The first step in the preparation process is to prepare a container for sintering. The container needs to be cleaned and dried to ensure that its internal environment is clean and free of impurities. Subsequently, ferric chloride hexahydrate is prepared as the raw material for the catalyst. Through grinding, the size of the ferric chloride hexahydrate particles becomes smaller, increasing the specific surface area of ​​the particles, which provides an ideal physical basis for subsequent uniform heating and sintering reactions.

[0063] In the second step, the ground ferric chloride hexahydrate powder is evenly dispersed in the container and the lid is covered to keep the reaction environment airtight. The container is placed in a heating device for precise temperature increase. During the sintering reaction, ferric chloride hexahydrate decomposes and oxidizes at high temperatures to generate Fe8O8(OH)8Cl 1.35 The temperature rise process is strictly controlled to ensure that the reaction is sufficient and no impurities are introduced, and the chloride and oxide formed can be fully combined.

[0064] The third step is to cool the product to room temperature after sintering. This step is extremely important. Rapid cooling will cause changes in the product structure or cracks, while slow cooling ensures the stability of the material structure. The product obtained after cooling is a muddy substance containing incompletely reacted by-products and residual reactants.

[0065] In the fourth step, the cooled sludge product is repeatedly washed with appropriate deionized water to remove residual chloride and other impurities. The washed product needs to be dried to remove moisture and ensure the purity and structural integrity of the catalyst. The final Fe8O8(OH)8Cl 1.35 The catalyst has excellent physical and chemical properties and is suitable for a variety of catalytic reactions. This preparation method is simple and controllable, and can obtain Fe8O8(OH)8Cl with high catalytic performance in a relatively short time. 1.35 catalyst.

[0066] Example 1.

[0067] Weigh 3.0g of ferric chloride hexahydrate and grind it in a mortar. Add the ground powder into a corundum crucible, cover the crucible, and place it in a small muffle furnace. Heat it to 180°C at 10°C / min, calcine it at a constant temperature for 2 hours, and then cool it down naturally. After room temperature, take out the crucible, collect the brown mud at the bottom of the crucible, wash it with water, remove impurities, and then centrifuge it for enrichment. After repeated washing 3 times, the enriched khaki precipitate is placed in a blast drying oven at 60°C and dried for 12 hours.

[0068] Example 2.

[0069] Weigh 3.0g of ferric chloride hexahydrate and grind it in a mortar. Add the ground powder into a corundum crucible, cover the crucible, and place it in a small muffle furnace. Raise the temperature to 200°C at 10°C / min, calcine at a constant temperature for 2 hours, and then cool naturally. After reaching room temperature, take out the crucible, collect the brown mud at the bottom of the crucible, wash it with water, remove impurities, and then centrifuge it for enrichment. After repeated washing for 3 times, place the enriched khaki precipitate in a blast drying oven at 60°C and dry it for 12 hours.

[0070] Example 3.

[0071] Weigh 3.0g of ferric chloride hexahydrate and grind it in a mortar. Add the ground powder into a corundum crucible, cover the crucible, and place it in a small muffle furnace. Heat it to 220°C at 10°C / min, calcine it at a constant temperature for 2 hours, and then cool it down naturally. After room temperature, take out the crucible, collect the brown mud at the bottom of the crucible, wash it with water, remove impurities, and then centrifuge it for enrichment. After repeated washing 3 times, the enriched khaki precipitate is placed in a blast drying oven at 60°C and dried for 12 hours.

[0072] Example 4.

[0073] Weigh 3.0g of ferric chloride hexahydrate and grind it in a mortar. Add the ground powder into a corundum crucible, cover the crucible, and place it in a small muffle furnace. Heat it to 240°C at 10°C / min, calcine it at a constant temperature for 2 hours, and then cool it down naturally. After room temperature, take out the crucible, collect the brown mud at the bottom of the crucible, wash it with water, remove impurities, and then centrifuge it for enrichment. After repeated washing for 3 times, the enriched khaki precipitate is placed in a blast drying oven at 60°C and dried for 12 hours.

[0074] Fe8O8(OH)8Cl prepared in Example 1-4 1.35 Photocatalysts are used to test the performance of photocatalytic water decomposition.

[0075] 20 mg of catalyst powder was added to the photocatalytic reactor, and then 20 mL of an appropriate deionized water solution containing 10% methanol was added thereto, stirring was continued, and nitrogen was bubbled for 60 minutes to remove oxygen in the system, then the nitrogen was stopped and the reactor was sealed, and a xenon light source simulating natural light was placed above the reactor, and the photocatalytic reaction was started when the xenon lamp was turned on. The gas produced by water decomposition in the system was sampled and analyzed at regular intervals using the gas chromatography provided by the photocatalytic system, with sampling once every 0.5 hours, and each sample was sampled and analyzed 5 times to determine the types and contents of gas products of the photocatalytic water decomposition reaction.

[0076] Figure 5 It is Fe8O8(OH)8Cl provided in Examples 1-4 of the present invention. 1.35 The photocatalytic hydrogen production performance diagram of the catalyst shows that Examples 1-4 all have relatively stable photocatalytic hydrogen production performance, among which Fe8O8(OH)8Cl prepared in Example 3 1.35 The photocatalyst can produce hydrogen by photolysis of water up to 2.05 μmol g -1 h -1 .

[0077] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. Fe8O8(OH)8Cl 1.35 The method for preparing a catalyst is characterized in that: The following steps are involved: (1) Grinding ferric chloride hexahydrate raw material; (2) placing the ground ferric chloride hexahydrate powder with uniform particles in a container, and then placing the ferric chloride hexahydrate powder in a heating device, setting a temperature rising program, and sintering; (3) The temperature is lowered to room temperature, the sludge product obtained by sintering is cleaned, and the cleaned product is dried to obtain Fe8O8(OH)8Cl 1.35 catalyst.

2. Fe8O8(OH)8Cl as claimed in claim 1 1.35 The method for preparing a catalyst is characterized in that: In step (1), the ferric chloride hexahydrate raw material is ground in a dry environment to prevent the raw material from hydrolysis.

3. Fe8O8(OH)8Cl as claimed in claim 1 1.35 The method for preparing a catalyst is characterized in that: In step (2), the container is loaded with raw materials in an amount greater than half of the volume of the container.

4. Fe8O8(OH)8Cl as claimed in claim 1 1.35 The method for preparing a catalyst is characterized in that: In step (2), the programmed heating rate is 10 °C / min, and the calcination temperature is maintained at 160-280 °C.

5. Fe8O8(OH)8Cl as claimed in claim 1 1.35 The method for preparing a catalyst is characterized in that: In step (2), the sintering working atmosphere is air.

6. Fe8O8(OH)8Cl as claimed in claim 1 1.35 The method for preparing a catalyst is characterized in that: In step (3), ultrasonic cleaning is performed with deionized water for 3 times, and the mixture is dried and collected after centrifugation.

7. Fe8O8(OH)8Cl as claimed in any one of claims 1 to 6 1.35 Catalyst preparation method Fe8O8(OH)8Cl prepared 1.35 A catalyst, characterized in that The microstructure is a rod-like cluster structure composed of nanoparticles, and the average particle size of a single nanorod is 50-100 nm.

8. Fe8O8(OH)8Cl as claimed in claim 7 1.35 The catalyst is used for photocatalytic hydrogen production.

Citation Information

Patent Citations

  • Preparation method of FeOCl

    CN102491429A

  • One-step synthesis of nanometer layered porous material of FeOCl and application thereof

    CN106698525A

  • Preparation method of porous rodlike Fe21.34O32 / C nanorod composite material

    CN113332983A

  • Fe-Fe3O4-FeP / g-C3N4 photocatalyst as well as preparation method and application thereof

    CN115869973A

  • METHOD OF DISPOSAL OF SPENT ETCHING SOLUTIONS CONTAINING IRON (II) SULFATES AND CHLORIDES

    RU2010101213A