Water permeable brick as well as preparation method and application thereof
By using specific proportions and particle sizes of steel slag and construction waste aggregate in permeable bricks, combined with basalt fibers, cement and other materials, the problem of insufficient permeability and strength of permeable bricks in the existing technology is solved, and high strength and high strength are achieved Water permeability effect.
Patent Information
- Application Number
- CN202411110100.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, permeability and strength of permeability and strength of permeability bricks prepared by composite steel slag and construction waste are low, making it difficult to meet the demand for high permeability and high-strength pavement floor tiles in sponge urban construction and green building materials policies.
Use steel slag aggregate and construction waste aggregate to match in specific proportions and particle sizes, and add basalt fibers, cement, silicon fume, thickener and water reducing agent to improve the strength and water permeability of permeable bricks through saturated water treatment and molding and maintenance technology. performance.
The compressive strength of permeable bricks exceeds 27.1MPa, the flexural strength exceeds 5.2MPa and the water permeability coefficient exceeds 2.5mm/s, which significantly improves the performance of permeable bricks.
Smart Images

Figure BDA0004992477070000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building engineering materials, and in particular to a permeable brick and a preparation method and application thereof. Background Art
[0002] Based on the actual needs of the national sponge city construction and development and the policy orientation of promoting "green building materials", the use of waste to prepare highly permeable and high-strength road and floor tile products has great practical significance. Steel slag is used as raw material, and the high calcium, high silicon, and high strength of steel slag are used to achieve the compressive and flexural strength required for permeable bricks, but its permeability is poor; permeable bricks are prepared from construction waste, so that they have good permeability, but their strength is low; in the prior art, steel slag and construction waste are generally compounded to prepare permeable bricks, but the permeability and strength of the prepared permeable bricks are still low. Therefore, there is an urgent need for a permeable brick with better strength and permeability. Summary of the invention
[0003] The purpose of the present invention is to provide a water-permeable brick and a preparation method and application thereof. The water-permeable brick provided by the present invention has better water permeability and strength.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a permeable brick, which comprises the following components by weight: 1575-2025 parts of steel slag aggregate, 225-675 parts of construction waste aggregate, 390-400 parts of cement, 20-25 parts of silica fume, 1-3 parts of basalt fiber, 2-3 parts of thickener, 1-1.5 parts of water reducer and 100-120 parts of water; the particle sizes of the steel slag aggregate and the construction waste aggregate are independently 1.18-9.5 mm; the length of the basalt fiber is 5-7 mm; the diameter of the basalt fiber is 7-25 μm.
[0006] Preferably, the steel slag aggregate includes steel slag coarse aggregate and steel slag fine aggregate.
[0007] Preferably, the particle size of the steel slag coarse aggregate is 4.75-9.5 mm; the particle size of the steel slag fine aggregate is 1.18-4.749 mm.
[0008] Preferably, the volume ratio of the steel slag coarse aggregate to the steel slag fine aggregate is (0.5-1.5):1.
[0009] Preferably, the construction waste aggregate includes construction waste coarse aggregate and construction waste fine aggregate.
[0010] Preferably, the particle size of the construction waste coarse aggregate is 4.75-9.5 mm; the particle size of the construction waste fine aggregate is 1.18-4.749 mm.
[0011] Preferably, the volume ratio of the coarse aggregate from construction waste to the fine aggregate from construction waste is (0.5-1.5):1.
[0012] Preferably, the thickening agent comprises hydroxypropyl methylcellulose.
[0013] The present invention also provides a method for preparing the permeable bricks described in the above technical solution, comprising the following steps:
[0014] (1) subjecting steel slag aggregate and construction waste aggregate to saturated water treatment to obtain treated steel slag aggregate and construction waste aggregate;
[0015] (2) mixing the treated steel slag aggregate and construction waste aggregate obtained in step (1), basalt fiber, water, cement, silica fume, a water reducing agent and a thickener to obtain a mixture;
[0016] (3) The mixture obtained in step (2) is molded and cured in sequence to obtain a permeable brick.
[0017] The present invention also provides the use of the permeable bricks described in the above technical solution or the permeable bricks prepared according to the preparation method described in the above technical solution in the field of construction.
[0018] The present invention provides a permeable brick, which comprises the following components by weight: 1575-2025 parts of steel slag aggregate, 225-675 parts of construction waste aggregate, 390-400 parts of cement, 20-25 parts of silica fume, 1-3 parts of basalt fiber, 2-3 parts of thickener, 1-1.5 parts of water reducer and 100-120 parts of water; the particle sizes of the steel slag aggregate and the construction waste aggregate are independently 1.18-9.5 mm; the length of the basalt fiber is 5-7 mm; the diameter of the basalt fiber is 7-25 μm. The permeable brick of the present invention uses steel slag and construction waste as aggregates. The steel slag has high hardness and wear resistance, and the construction waste has good permeability. The particle sizes of the two are controlled, and the two are filled and inlaid with each other, and rotate and displace in parallel. Under the mutual extrusion stress, a synergistic stress effect is exerted to improve the strength and permeability of the permeable brick; hydrophobic basalt fiber is added and its length and diameter are controlled to further improve the strength and permeability of the permeable brick; silica fume is added to improve the strength and density of the permeable brick, and improve the fluidity and workability of the permeable brick; a thickener is added to thicken and retain water to prevent cement slurry from segregating and bleeding; the composition and dosage of each component are controlled, and each component cooperates to improve the strength and permeability of the permeable brick. The results of the embodiment show that the compressive strength of the permeable brick provided by the present invention is above 27.1MPa, the flexural strength is above 5.2MPa, and the permeability coefficient is above 2.5mm / s. DETAILED DESCRIPTION
[0019] The present invention provides a permeable brick, which comprises the following components by weight: 1575-2025 parts of steel slag aggregate, 225-675 parts of construction waste aggregate, 390-400 parts of cement, 20-25 parts of silica fume, 1-3 parts of basalt fiber, 2-3 parts of thickener, 1-1.5 parts of water reducer and 100-120 parts of water.
[0020] Unless otherwise specified, the present invention has no particular limitation on the sources of the components, and commercially available products or conventional products known to those skilled in the art may be used.
[0021] The permeable brick provided by the present invention comprises 1575-2025 parts of steel slag aggregate, preferably 1800-2025 parts by weight. In the present invention, the steel slag is a byproduct produced in the steel smelting process, mainly composed of iron oxide, silicon oxide, calcium oxide, etc. and a small amount of metal elements, has high hardness and wear resistance, and can be used in permeable bricks to exert strength and water permeability, while making steel slag solid waste resource utilization.
[0022] In the present invention, the particle size of the steel slag aggregate is 1.18-9.5 mm.
[0023] In the present invention, the steel slag aggregate preferably includes steel slag coarse aggregate and steel slag fine aggregate; the particle size of the steel slag coarse aggregate is preferably 4.75-9.5 mm; the particle size of the steel slag fine aggregate is preferably 1.18-4.749 mm; the volume ratio of the steel slag coarse aggregate to the steel slag fine aggregate is preferably (0.5-1.5):1, more preferably 1:1. The present invention limits the amount, composition and particle size of the steel slag aggregate to the above range, which can cooperate with the construction waste aggregate to further improve the strength and permeability of the permeable brick.
[0024] Based on the mass of steel slag aggregate being 1575 to 2025 parts, the permeable brick provided by the present invention comprises 225 to 675 parts of construction waste aggregate, preferably 225 to 450 parts. In the present invention, the construction waste aggregate is preferably construction waste generated during demolition, renovation or construction, and more preferably at least one of waste concrete, bricks and stones. The addition of construction waste aggregate and steel slag aggregate in the present invention can improve the permeability and strength of the permeable brick.
[0025] In the present invention, the particle size of the construction waste aggregate is 1.18-9.5 mm.
[0026] In the present invention, the construction waste aggregate preferably includes coarse aggregate and fine aggregate; the particle size of the coarse aggregate is preferably 4.75-9.5 mm; the particle size of the fine aggregate is preferably 1.18-4.749 mm; the volume ratio of the coarse aggregate to the fine aggregate is preferably (0.5-1.5):1, more preferably 1:1. The present invention limits the amount, composition and particle size of the construction waste aggregate to the above range, which can cooperate with the steel slag aggregate to further improve the strength and permeability of the permeable brick.
[0027] Based on 1575-2025 parts of steel slag aggregate, the permeable brick provided by the present invention includes 390-400 parts of cement, preferably 395-400 parts, and more preferably 398 parts. In the present invention, the cement is used as a cementitious material to improve the strength of the permeable brick.
[0028] In the present invention, the cement is preferably ordinary Portland cement with a grade of 42.5. The present invention limits the amount of cement to the above range, which can further improve the strength and water permeability of the permeable brick.
[0029] Based on the mass of steel slag aggregate being 1575 to 2025 parts, the permeable brick provided by the present invention includes 20 to 25 parts of silica fume, preferably 21 to 24 parts. In the present invention, the silica fume can improve the strength, density, and durability of the permeable brick, and improve the fluidity and workability during the preparation of the permeable brick. The present invention limits the amount of silica fume to the above range, which can further improve the strength and permeability of the permeable brick.
[0030] Based on the mass of steel slag aggregate being 1575 to 2025 parts, the permeable brick provided by the present invention comprises 1 to 3 parts of basalt fiber, preferably 2 parts. The addition of basalt fiber in the present invention can cooperate with other components to increase the porosity of the permeable brick and the connectivity of the pores, thereby increasing the strength and water permeability of the permeable brick; at the same time, basalt fiber is a hydrophobic fiber, which can improve the durability of the permeable brick compared with hydrophilic fiber, and has lower cost compared with carbon fiber.
[0031] In the present invention, the length of the basalt fiber is 5-7 mm, preferably 6 mm; the diameter of the basalt fiber is 7-25 μm, preferably 17 μm. The present invention limits the length and diameter of the basalt fiber to the above range, which can further improve the strength and water permeability of the permeable brick.
[0032] In the present invention, the density of the basalt fiber is preferably 2 to 3 g / cm 3 , more preferably 2.65 g / cm 3The tensile strength of the basalt fiber is preferably 1200-1300 MPa, more preferably 1256 MPa; the elastic modulus of the basalt fiber is preferably 76-80 GPa, more preferably 76-78 GPa, and further preferably 76.1 GPa. The present invention limits the density and other parameters of the basalt fiber to the above range, which can further improve the strength and permeability of the permeable brick.
[0033] Based on 1575 to 2025 parts by mass of steel slag aggregate, the permeable brick provided by the present invention includes 2 to 3 parts of thickener, preferably 2.5 parts.
[0034] In the present invention, the thickener is preferably hydroxypropyl methylcellulose. In the present invention, the thickener is used for thickening and water retention. Under the condition of high water-cement ratio, it can prevent cement slurry from segregating and bleeding, increase the bonding force of the matrix, improve the uniformity and hardening ability of the matrix material, improve the viscoelasticity, fluidity and water retention of basalt fiber freshly mixed steel slag and construction waste mixed aggregate concrete, and improve the strength of permeable bricks.
[0035] In the present invention, the density of the hydroxypropyl methylcellulose is preferably 950 to 1000 kg / m 3 , more preferably 980kg / m 3 The viscosity of the hydroxypropyl methylcellulose is preferably 150,000 to 250,000 Pa·s, more preferably 200,000 Pa·s; the fineness of the hydroxypropyl methylcellulose is preferably >80 mesh. The present invention limits the amount of thickener and other parameters within the above range, which can further improve the strength and water permeability of the permeable brick.
[0036] Based on 1575 to 2025 parts by mass of steel slag aggregate, the permeable brick provided by the present invention includes 1 to 1.5 parts of water reducing agent, preferably 1.1 to 1.4 parts.
[0037] In the present invention, the water reducer preferably includes a lignin-based water reducer, a naphthalene-based water reducer or a polycarboxylic acid-based high-performance water reducer. The present invention limits the type and amount of the water reducer to the above range, which can further improve the fluidity of each component, thereby further improving the strength and water permeability of the permeable brick.
[0038] Based on the mass of steel slag aggregate being 1575 to 2025 parts, the permeable brick provided by the present invention comprises 100 to 120 parts of water, preferably 105 to 115 parts, and more preferably 109 parts. The present invention limits the amount of water to the above range, so that the permeable brick has a suitable water-binder ratio, and further improves the strength and water permeability of the permeable brick.
[0039] The invention controls the composition and dosage of each component, and the components cooperate to improve the strength and water permeability of the permeable brick, while making use of steel slag and construction waste as resources, thereby saving energy and protecting the environment.
[0040] The present invention also provides a method for preparing the permeable bricks described in the above technical solution, comprising the following steps:
[0041] (1) subjecting steel slag aggregate and construction waste aggregate to saturated water treatment to obtain treated steel slag aggregate and construction waste aggregate;
[0042] (2) mixing the treated steel slag aggregate and construction waste aggregate obtained in step (1), basalt fiber, water, cement, silica fume, a water reducing agent and a thickener to obtain a mixture;
[0043] (3) The mixture obtained in step (2) is molded and cured in sequence to obtain a permeable brick.
[0044] The present invention performs saturated water treatment on steel slag aggregate and construction waste aggregate to obtain treated steel slag aggregate and construction waste aggregate. In the present invention, the saturated water treatment can prevent the aggregate from absorbing water when the components are subsequently mixed with water, causing uneven mixing of the components.
[0045] The present invention preferably soaks the steel slag aggregate and the construction waste aggregate in water for saturation treatment. In the present invention, the amount of water used for the steel slag aggregate and the construction waste aggregate for saturation treatment is not included in the amount of water used for the permeable bricks described in the above technical solution.
[0046] The present invention has no special limitation on the amount of water used in the saturation treatment, as long as the amount of water can saturate the steel slag aggregate and the construction waste aggregate.
[0047] In the present invention, the time of the saturated water treatment is preferably 1 to 1.5 hours.
[0048] After the saturated water treatment is completed, the present invention preferably dries the saturated water treated steel slag aggregate and construction waste aggregate to obtain treated steel slag aggregate and construction waste aggregate.
[0049] In the present invention, the drying is preferably air-drying. The present invention has no special limitation on the operation of air-drying, as long as the surface of the steel slag aggregate and the construction waste aggregate is dry.
[0050] After obtaining the treated steel slag aggregate and construction waste aggregate, the present invention mixes the treated steel slag aggregate and construction waste aggregate, basalt fiber, water, cement, silica fume, a water reducing agent and a thickener to obtain a mixture.
[0051] In the present invention, the mixing of the treated steel slag aggregate and construction waste aggregate, basalt fiber, water, cement, silica fume, water reducer and thickener is preferably as follows: under stirring conditions, basalt fiber is sprinkled into the treated steel slag aggregate and construction waste aggregate, and then part of the water is added and stirred for 1 to 2 minutes, and then cement, silica fume, water reducer, thickener and remaining water are added and stirred for 1 to 2 minutes.
[0052] In the present invention, the mass of the partial water is preferably 0.4 to 0.6 of the total mass of water, and more preferably 0.5. The mixing method of the present invention can make the components mixed more uniformly.
[0053] After obtaining the mixture, the present invention sequentially shapes and cures the mixture to obtain a permeable brick.
[0054] In the present invention, the molding is preferably performed in a mold. The present invention has no special limitation on the size of the mold, which can be selected according to actual needs.
[0055] In the present invention, it is preferred to manually vibrate the mixture for 5 to 15 seconds when the mixture is filled to 3 / 6 to 5 / 6 of the total volume of the mold, and then fill the mold and perform static pressing; more preferably, it is manually vibrated for 10 seconds when the mixture is filled to 2 / 3 of the total volume of the mold, and then fill the mold and perform static pressing.
[0056] The present invention has no special limitation on the operation of the artificial vibration, and the technical solution of artificial vibration well known to those skilled in the art can be adopted.
[0057] In the present invention, the static pressure is preferably 10-20 MPa, more preferably 15 MPa; the static pressure time is preferably 80-100 s, more preferably 90 s. The molding method of the present invention can improve the density of the permeable brick, and further improve the strength and permeability of the permeable brick.
[0058] In the present invention, the curing is preferably: curing for 20 to 26 hours under standard curing conditions, then removing the mold, and then immersing in water for curing to a specified age; more preferably: curing for 24 hours under standard curing conditions, then removing the mold, and then immersing in water for curing to 28 days.
[0059] The present invention has no special limitation on the amount of water used during the curing process, as long as the amount of water can cover the water-permeable bricks. The curing method of the present invention can further improve the strength and water permeability of the water-permeable bricks.
[0060] The present invention also provides the use of the permeable bricks described in the above technical solution or the permeable bricks prepared according to the preparation method described in the above technical solution in the field of construction.
[0061] The present invention has no special limitation on the operation of the application, and the technical solutions of the application well known to those skilled in the art may be adopted.
[0062] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Example 1
[0064] A permeable brick, composed of the following components by weight: 2025 parts of steel slag aggregate, 225 parts of construction waste aggregate, 398 parts of cement, 21 parts of silica fume, 2 parts of basalt fiber, 2.5 parts of hydroxypropyl methylcellulose (density 980kg / m 3 , viscosity of 200000Pa·s, fineness>80 mesh), 1.1 parts of polycarboxylic acid high-performance water reducer and 109 parts of water; the basalt fiber has a length of 6mm, a diameter of 17μm, and a density of 2.65g / cm 3 , tensile strength is 1256MPa, elastic modulus is 76.1GPa; the steel slag aggregate is formed by mixing steel slag coarse aggregate (4.75-9.5mm) and steel slag fine aggregate (1.18-4.749mm) in a volume ratio of 1:1; the construction waste aggregate is formed by mixing construction waste coarse aggregate (4.75-9.5mm) and construction waste fine aggregate (1.18-4.749mm) in a volume ratio of 1:1;
[0065] The preparation method of the permeable brick is:
[0066] (1) putting steel slag aggregate and construction waste aggregate into water and soaking them for 1 hour for saturation treatment, and then drying them in the sun until the surface is dry, so as to obtain treated steel slag aggregate and construction waste aggregate;
[0067] (2) placing the treated steel slag aggregate and construction waste aggregate in step (1) into a mixer, evenly sprinkling basalt fiber into the mixer while stirring, adding half the weight of water, stirring for 1.5 min, then adding cement, silica fume, water reducing agent, hydroxypropyl methylcellulose and the remaining water, stirring for 1.5 min, and obtaining a mixture;
[0068] (3) The mixture obtained in step (2) is filled into a mold. When the volume reaches 2 / 3, it is manually vibrated for 10 seconds, then filled, and mechanical static pressure is applied for 90 seconds with a static pressure of 15 MPa. It is placed under standard curing conditions for 24 hours. After the mold is removed, it is placed in a curing pool and soaked in water for curing for 28 days to obtain a permeable brick.
[0069] Example 2
[0070] A permeable brick, composed of the following components by weight: 1800 parts of steel slag aggregate, 450 parts of construction waste aggregate, 398 parts of cement, 21 parts of silica fume, 2 parts of basalt fiber, 2.5 parts of hydroxypropyl methylcellulose (density 980kg / m 3 , viscosity of 200000Pa·s, fineness>80 mesh), 1.1 parts of polycarboxylic acid high-performance water reducer and 109 parts of water; the basalt fiber has a length of 6mm, a diameter of 17μm, and a density of 2.65g / cm 3 , tensile strength is 1256MPa, elastic modulus is 76.1GPa; the steel slag aggregate is formed by mixing steel slag coarse aggregate (4.75-9.5mm) and steel slag fine aggregate (1.18-4.749mm) in a volume ratio of 1:1; the construction waste aggregate is formed by mixing construction waste coarse aggregate (4.75-9.5mm) and construction waste fine aggregate (1.18-4.749mm) in a volume ratio of 1:1;
[0071] The preparation method of the permeable brick is the same as that of Example 1.
[0072] Example 3
[0073] A permeable brick, composed of the following components by weight: 1575 parts of steel slag aggregate, 675 parts of construction waste aggregate, 398 parts of cement, 21 parts of silica fume, 2 parts of basalt fiber, 2.5 parts of hydroxypropyl methylcellulose (density 980kg / m 3 , viscosity of 200000Pa·s, fineness>80 mesh), 1.1 parts of polycarboxylic acid high-performance water reducer and 109 parts of water; the basalt fiber has a length of 6mm, a diameter of 17μm, and a density of 2.65g / cm 3 , tensile strength is 1256MPa, elastic modulus is 76.1GPa; the steel slag aggregate is formed by mixing steel slag coarse aggregate (4.75-9.5mm) and steel slag fine aggregate (1.18-4.749mm) in a volume ratio of 1:1; the construction waste aggregate is formed by mixing construction waste coarse aggregate (4.75-9.5mm) and construction waste fine aggregate (1.18-4.749mm) in a volume ratio of 1:1;
[0074] The preparation method of the permeable brick is the same as that of Example 1.
[0075] The bulk density, compressive strength (the size of the permeable brick is 200mm×100mm×60mm), flexural strength (the size of the permeable brick is 200mm×100mm×60mm) and permeability coefficient (the size of the permeable brick is radius R=100mm, height h=50mm) of the permeable bricks in Examples 1 to 3 were tested according to GB / T 4111-2013 "Test methods for concrete blocks and bricks". The results are shown in Table 1.
[0076] Table 1 Bulk density, compressive strength, flexural strength and water permeability coefficient of permeable bricks in Examples 1 to 3
[0077]
[0078] It can be seen from Table 1 that the permeable brick provided by the present invention has excellent compressive strength, flexural strength and water permeability coefficient.
[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A permeable brick, comprising the following components by weight: 1575-2025 parts of steel slag aggregate, 225-675 parts of construction waste aggregate, 390-400 parts of cement, 20-25 parts of silica fume, 1-3 parts of basalt fiber, 2-3 parts of thickener, 1-1.5 parts of water reducer and 100-120 parts of water; the particle sizes of the steel slag aggregate and the construction waste aggregate are independently 1.18-9.5 mm; the length of the basalt fiber is 5-7 mm; the diameter of the basalt fiber is 7-25 μm.
2. The permeable brick according to claim 1, characterized in that: The steel slag aggregate includes steel slag coarse aggregate and steel slag fine aggregate.
3. The permeable brick according to claim 2, characterized in that: The particle size of the steel slag coarse aggregate is 4.75-9.5 mm; the particle size of the steel slag fine aggregate is 1.18-4.749 mm.
4. The permeable brick according to claim 2 or 3, characterized in that: The volume ratio of the steel slag coarse aggregate to the steel slag fine aggregate is (0.5-1.5):
1.
5. The permeable brick according to claim 1, characterized in that: The construction waste aggregate includes construction waste coarse aggregate and construction waste fine aggregate.
6. The permeable brick according to claim 5, characterized in that: The particle size of the coarse aggregate of construction waste is 4.75-9.5 mm; the particle size of the fine aggregate of construction waste is 1.18-4.749 mm.
7. The permeable brick according to claim 5 or 6, characterized in that: The volume ratio of the coarse aggregate of construction waste to the fine aggregate of construction waste is (0.5-1.5):
1.
8. The permeable brick according to claim 1, characterized in that: The thickening agent includes hydroxypropyl methylcellulose.
9. The method for preparing the permeable brick according to any one of claims 1 to 8, comprising the following steps: (1) subjecting steel slag aggregate and construction waste aggregate to saturated water treatment to obtain treated steel slag aggregate and construction waste aggregate; (2) mixing the treated steel slag aggregate and construction waste aggregate obtained in step (1), basalt fiber, water, cement, silica fume, a water reducing agent and a thickener to obtain a mixture; (3) The mixture obtained in step (2) is molded and cured in sequence to obtain a permeable brick.
10. Use of the permeable brick according to any one of claims 1 to 8 or the permeable brick prepared by the preparation method according to claim 9 in the field of construction.
Citation Information
Patent Citations
Anti-frost environment-friendly water permeable brick and preparing method thereof
CN109626902A
Water-permeable concrete material and preparation method thereof
CN110981364A
Method for preparing high-strength and high-permeability concrete from hexagonal boron nitride and basalt fiber