Cerium oxide / yttrium oxide composite stabilized zirconium oxide grinding medium and preparation method thereof

Through the preparation method of cerium oxide/yttrium oxide composite stable zirconia grinding medium, combined with spray drying and rolling molding technology, the aging problem of yttrium oxide stable tetragonal zirconia ceramics in low temperature environments is solved, and high density and wear resistance are achieved , reduces sintering temperature and production costs.

CN119038989AActive Publication Date: 2024-11-29ZHEJIANG JINKUN XILI ZIRCONIUM BEAD CO LTD

Patent Information

Application Number
CN202411545029.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29
Estimated Expiration
2044-11-01

AI Technical Summary

Technical Problem

Existing yttrium zirconia ceramics are prone to aging in low temperature and humid environments, and the single stabilizer zirconia ceramics have problems of wear resistance and high cost in the application of grinding media. How to ensure the anti-aging performance while reducing sintering Temperature and production costs are challenges.

Method used

Using cerium oxide/yttrium oxide composite stable zirconia grinding medium, mix zirconia, cerium oxide, yttrium oxide and kaolin, add dispersant and binder for spray drying and rolling molding, sintering at low temperature and polishing, control particle size and sintering aids are added to improve density and anti-aging properties.

Benefits of technology

It achieves high density tetragonal phase zirconia under low temperature conditions, extends service life, reduces production costs, and improves wear resistance and anti-aging properties of the grinding medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038989A_ABST
    Figure CN119038989A_ABST
Patent Text Reader

Abstract

The invention provides a cerium oxide / yttrium oxide composite stabilized zirconium oxide grinding medium and a preparation method thereof, and the method comprises the following steps: 1, mixing zirconium oxide, cerium oxide, yttrium oxide and kaolin, adding a proper amount of a dispersant and water, and grinding to obtain slurry; 2, carrying out centrifugal spray drying on the slurry to obtain cerium oxide / yttrium oxide composite stable zirconium oxide powder; step 3, adding a binder into the cerium oxide / yttrium oxide composite stabilized zirconia powder, and carrying out rolling forming to prepare a spherical grinding medium green body; and 4, sintering and polishing the spherical grinding medium green body to obtain the cerium oxide / yttrium oxide composite stable zirconium oxide grinding medium. According to the method, low particle size and high specific surface are obtained through high-temperature ball milling, and the stabilizer is promoted to be dissolved in zirconium oxide crystal lattices through heat treatment, so that the sintering activity is improved, the sintering temperature is reduced, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zirconium oxide ceramics, and in particular to a cerium oxide / yttria composite stabilized zirconium oxide grinding medium and a preparation method thereof. Background Art

[0002] Tetragonal zirconia ceramics (TZP) are the most representative ceramics, which are widely used in various fields due to their advantages of high strength, high hardness, high fracture toughness and good biocompatibility. Among them, tetragonal zirconia as a grinding medium has excellent wear resistance and is widely used in coatings, inks and positive electrode material grinding.

[0003] Yttria-stabilized tetragonal zirconia ceramics (Y-TZP) are the most studied TZP materials. The yttria content is crucial to the performance of zirconia ceramics. For example, when the yttria content is less than 2 mol%, it is difficult to obtain tetragonal zirconia with a high content. The toughness of the material is best when the content is 2 mol%, and the strength of the material is highest when the content is between 2 and 3 mol%. However, when Y-TZP is used in a low-temperature and humid environment, especially in the temperature range of 65-400°C, it is very easy to age at low temperatures, which is mainly manifested as microscopic or macroscopic microcracks on the surface, which affects the mechanical properties of the material to a certain extent and limits its application in special environments. Therefore, it is very important to prevent Y-TZP from aging at low temperatures. TZP ceramics with CeO2 as a stabilizer have excellent fracture toughness and anti-aging properties, but compared with Y-TZP, the densification of Ce-TZP requires a higher sintering temperature and a longer holding time, and the Ce-TZP grains are coarser, so the strength and hardness are also low.

[0004] ZrO2 ceramics stabilized by a single stabilizer have certain limitations in practical applications. By adding two or more stabilizers to the ZrO2 matrix, ZrO2 composite ceramics with better comprehensive performance can be obtained. Many scholars have also conducted a series of studies on zirconia ceramics stabilized by multiple stabilizers. In "Low-temperature Aging of YCe-TZP Ceramics", Yin Bangyue et al. prepared YCe-TZP ceramics with different proportions by co-precipitation process, and carried out low-temperature aging test after sintering at 1450℃. Among them, 3Y4Ce-TZP hardly experienced aging phenomenon; during the aging process, a CeO2 protective layer was formed on the surface of 3Y4Ce-TZP to prevent the formation of Y-OH bonds, thereby effectively inhibiting the t (tetragonal phase) → m (monoclinic phase) aging phase transition. However, due to the introduction of cerium oxide as a stabilizer, the sintering temperature of zirconia is higher, and some mechanical properties are reduced, which affects its wear resistance when used as a grinding medium. At present, there are few reports on the application of cerium oxide and yttrium oxide composite stabilized zirconia materials in grinding media. How to ensure that it has excellent low-temperature aging resistance and wear resistance is a crucial point in promoting its application in the field of grinding media. The sintering of grinding media is also the link with the largest energy consumption, so reducing the sintering temperature is also a research focus of zirconia grinding media. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention provides a cerium oxide / yttria composite stabilized zirconia grinding medium and a preparation method thereof, which can be sintered at low temperature to be dense, and at the same time has excellent anti-aging and wear resistance. The cerium oxide and yttria composite stabilized zirconia grinding medium and a preparation method thereof extend its service life and reduce production costs.

[0006] To achieve the above object, the present invention provides a cerium oxide / yttria composite stabilized zirconium oxide grinding medium and a preparation method thereof, wherein the preparation method is as follows: Step 1: zirconium oxide, cerium oxide, yttrium oxide and kaolin are mixed in a certain proportion, and then a proper amount of dispersant and deionized water are added to grind to obtain a uniformly mixed slurry; Step 2: The mixed slurry is centrifugally spray-dried to obtain cerium oxide and yttrium oxide composite stabilized zirconium oxide powder; the spray drying atomizing disk speed is 9000-11000r / min, the inlet temperature is 240-260°C, and the outlet temperature is 95-110°C, so as to ensure that the granulated powder has good sphericity and fluidity; Step 3, adding cerium oxide and yttrium oxide composite stabilized zirconium oxide powder to a binder and rolling-molding to obtain a spherical grinding medium green body; Step 4: After sintering, the green body of the grinding medium is polished to obtain a cerium oxide and yttrium oxide composite stabilized zirconium oxide grinding medium.

[0007] Preferably, in step 1, the added amounts of zirconium oxide, cerium oxide, yttrium oxide and kaolin are 85-90wt%, 10-15wt%, 1-2wt% and 0.1-0.5wt%.

[0008] Preferably, in step 1, the added dispersant is Dolapix ce64, and the added amount is 0.5wt%.

[0009] Preferably, in step 1, the amount of deionized water added is 50 wt %, and the solid content of the slurry is 50 wt %.

[0010] Preferably, in step 1, the slurry temperature is maintained at 70-90°C during the grinding process.

[0011] Preferably, in step 1, the mixed slurry grinding particle size D50 is controlled in the range of 0.15-0.2 um.

[0012] Preferably, in step three, the molding process binder is a composition of PVA, glycerol and water.

[0013] Preferably, in step 4, the green body of the grinding medium is sintered by heating the green body to 1300-1350° C. at a heating rate of 2° C. / min, keeping the temperature for 2 hours under pressureless conditions in an air atmosphere, and then naturally cooling the green body to room temperature.

[0014] Preferably, in the step 4, the sintered grinding medium is polished by a sand mill at a line speed of 8 m / s, and the polishing material is white corundum with an addition amount of 2 wt%.

[0015] The beneficial effects of the present invention are as follows: The present invention obtains low particle size and high specific surface area through high temperature ball milling, and also promotes the solid solution of stabilizer into zirconium oxide lattice through heat treatment, thereby improving sintering activity. Stable tetragonal zirconium oxide can be obtained by sintering at low temperature (1300-1350℃), and the density is as high as 6.13-6.14g / m 3 . In the later stage, the surface roughness is reduced through polishing treatment. Combining the above properties, it has excellent wear resistance in the grinding process, the self-wear is less than 10ppm / h, and the service life is extended.

[0016] The present invention adopts a solid phase synthesis process, adds a small amount of yttrium oxide to the cerium oxide stabilized zirconia ceramic to improve the mechanical properties, and adds kaolin as a sintering aid; kaolin is mainly composed of aluminum oxide and silicon oxide, and is added to improve the sintering activity, reduce the sintering temperature, obtain excellent low-temperature aging resistance and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the X-ray diffraction pattern of Example 1 before aging; Figure 2This is the X-ray diffraction pattern of Example 1 after aging; Figure 3 This is the X-ray diffraction pattern of Example 2 before aging; Figure 4 This is the X-ray diffraction pattern after aging of Example 2; Figure 5 This is the X-ray diffraction pattern of Comparative Example 1 before aging; Figure 6 This is the X-ray diffraction pattern of comparative example 1 after aging; Figure 7 This is the X-ray diffraction pattern of Comparative Example 2 before aging; Figure 8 This is the X-ray diffraction pattern of comparative example 2 after aging; Fig. 9 This is the X-ray diffraction pattern of Comparative Example 3 before aging; Fig.10 This is the X-ray diffraction pattern of Comparative Example 3 after aging; Fig.11 This is the X-ray diffraction pattern of Comparative Example 4 before aging; Fig.12 This is the X-ray diffraction pattern of Comparative Example 4 after aging; Fig.13 This is the X-ray diffraction pattern of Comparative Example 5 before aging; Fig.14 This is the X-ray diffraction pattern of Comparative Example 5 after aging. DETAILED DESCRIPTION

[0018] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present application will be further described below in conjunction with specific embodiments.

[0019] The test method of the present invention is: 1. Grinding media density: Archimedes drainage method, 2. Grinding media wear: 1L sand mill, grinding media addition amount 2.6kg is recorded as m0, test in clean water at a linear speed of 12m / s for 20 hours is recorded as t, weigh and calculate weight loss, weight before test is recorded as m1, weight after test is recorded as m 2, ; 3. Phase content: X-ray diffractometer (XRD); 4. Low temperature anti-aging performance test: The sample is placed in a hydrothermal kettle, water is added to a filling rate of 80%, and hydrothermal treatment is performed at 200°C for 48 hours.

[0020] Embodiment 1: Zirconia, cerium oxide, yttrium oxide and kaolin were mixed in a ratio of 86.2wt%, 12wt%, 1.5wt% and 0.3wt%, and then pure water was added to a solid content of 50%. The mixture was ground using a drum ball mill, and 0.5wt% Dolapix ce64 was added as a dispersant. The temperature during the grinding process was controlled at about 80°C, and the mixture was ground to a particle size of D 50 =0.15um, the slurry was transferred to the granulation tower for spray granulation, the atomizing disk speed was 10000r / min, the inlet temperature was 250℃, and the outlet temperature was 105℃, to obtain cerium oxide and yttrium oxide composite stabilized zirconia powder.

[0021] The powder was added with a binder (PVA, glycerol, and deionized water were mixed in a ratio of 1:0.5:90) and rolled to prepare a green body of a grinding medium ball. The amount of the binder added was 8-10wt%. The green body was heated from room temperature to 1330°C in an air atmosphere at a rate of 2°C / min, kept warm for 2.5h, and then naturally cooled to room temperature. 2wt% white corundum was added and polished in a sand mill at a linear speed of 8m / s until the surface was smooth to obtain a finished product of a cerium oxide / yttria composite stabilized zirconium oxide grinding medium ball. The grinding medium density is 6.138g / m 3 The wear test result is 8.0ppm / h, and the tetragonal phase content is 100% after aging for 48h under hydrothermal conditions at 200℃. Figure 1 , Figure 2 1 and 2 are X-ray diffraction patterns of the grinding media before and after aging, respectively. The ordinate represents the relative intensity, and the abscissa represents the diffraction angle 2θ.

[0022] Embodiment 2: Zirconia, cerium oxide, yttrium oxide and kaolin were mixed in a ratio of 85wt%, 13.2wt%, 1.5wt% and 0.3wt%, and then pure water was added to a solid content of 50%. The mixture was ground in a drum ball mill, and 0.5wt% Dolapix ce64 (Zima Chemical CE64) was added as a dispersant. The temperature during the grinding process was controlled at about 80°C. When the particle size D50 was 0.15um, the slurry was transferred to a granulation tower for spray granulation. The atomizing disk speed was 10000r / min, the inlet temperature was 250°C, and the outlet temperature was 105°C, to obtain cerium oxide and yttrium oxide composite stabilized zirconia powder.

[0023] The powder was added with a binder (the binder was PVA, glycerol, and deionized water mixed in a ratio of 1:0.5:90) and rolled to prepare a green body of a grinding medium ball. The green body was heated from room temperature to 1330°C in an air atmosphere at a rate of 2°C / min, kept warm for 2.5 hours, and then naturally cooled to room temperature. 2wt% white corundum was added and polished in a sand mill at a linear speed of 8m / s until the surface was smooth to obtain a finished product of a cerium oxide / yttria composite stabilized zirconium oxide grinding medium ball. The grinding medium had a density of 6.140g / m3, a wear test result of 8.2ppm / h, and was aged for 48h under hydrothermal conditions at 200°C. The tetragonal phase content was 100%. Figure 3 , Figure 4 The figures are respectively the X-ray diffraction patterns of the grinding media before and after aging, in which the ordinate represents the relative intensity and the abscissa represents the diffraction angle 2θ.

[0024] Comparative Example 1: Compared with Example 1, zirconium oxide, cerium oxide, yttrium oxide and kaolin are mixed in a ratio of 86.2wt%, 13.5wt%, 0wt% and 0.3wt%, and the other conditions are the same. The grinding medium ball density is 5.967g / m3, the abrasion test result is 3961.4ppm / h, and the tetragonal phase content is 12% after aging for 48h under hydrothermal conditions at 200℃. Figure 5 , Figure 6 The figures are respectively the X-ray diffraction patterns of the grinding media before and after aging, in which the ordinate represents the relative intensity and the abscissa represents the diffraction angle 2θ.

[0025] Comparative Example 2: Compared with Example 1, zirconium oxide, cerium oxide, yttrium oxide and kaolin are mixed in a ratio of 86.5wt%, 12wt%, 1.5wt% and 0wt%, and the other conditions are the same. The grinding medium ball density is 6.055g / m3, the abrasion test result is 1807.0ppm / h, and the tetragonal phase content is 95% after aging for 48h under hydrothermal conditions at 200℃. Figure 7 , Figure 8 The figures are respectively the X-ray diffraction patterns of the grinding media before and after aging, in which the ordinate represents the relative intensity and the abscissa represents the diffraction angle 2θ.

[0026] Comparative Example 3: Compared with Example 1, 0.13wt% alumina and 0.17wt% silicon oxide were used to replace kaolin, and other conditions were the same. The grinding media was sintered at 1330°C and had a density of 6.101 g / m 3 The wear test result is 55.6ppm / h, and the tetragonal phase content is 100% after aging for 48h under 200℃ hydrothermal conditions. Fig. 9 , Fig.10The figures are respectively the X-ray diffraction patterns of the grinding media before and after aging, in which the ordinate represents the relative intensity and the abscissa represents the diffraction angle 2θ.

[0027] Comparative Example 4: Compared with Example 1, the powder grinding process temperature is controlled at about 30°C, and the other conditions are the same. The density of the obtained grinding medium ball is 6.109g / m3, the abrasion test result is 298.2ppm / h, and the tetragonal phase content is 92% after aging for 48h under 200°C hydrothermal conditions. Fig.11 , Fig.12 The figures are respectively the X-ray diffraction patterns of the grinding media before and after aging, in which the ordinate represents the relative intensity and the abscissa represents the diffraction angle 2θ.

[0028] Comparative Example 5: Compared with Example 1, the powder grinding process temperature was controlled at about 50°C, and other conditions were the same. The density of the obtained grinding medium ball was 6.120 g / m 3 The wear test result is 205.0ppm / h. After aging for 48h under 200℃ hydrothermal conditions, the tetragonal phase content is 94%. Fig.13 , Fig.14 The X-ray diffraction patterns of the grinding media before and after aging are shown in Figure 1. The ordinate represents the relative intensity, and the abscissa represents the diffraction angle 2θ. Table 1 Experimental parameters of various embodiments and comparative examples , Table 2 Performance test parameters of various embodiments and comparative examples .

[0029] From Example 1 and Comparative Example 1, the addition of yttrium oxide and cerium oxide composite stabilized zirconia helps to improve its wear resistance. This is because in the cerium oxide and yttrium oxide composite stabilized zirconia, Y 3+ Segregation at grain boundaries inhibits grain growth, improves the strength, hardness and density of Ce-TZP, and thus achieves excellent wear resistance.

[0030] From Example 1 and Comparative Examples 2 and 3, the addition of kaolin can be used as a sintering aid to accelerate the densification of zirconia and obtain high density. The main components of kaolin are aluminum oxide and silicon oxide, as well as a small amount of alkali metal oxides, which together act as sintering aids during the sintering process. Aluminum oxide inhibits grain growth, and silicon oxide easily forms a eutectic liquid phase with the stabilizer of ZrO2 ceramics, thereby improving the efficiency of sintering mass transfer, promoting the densification of ceramics, and thus affecting the mechanical properties of ceramics.

[0031] From Example 1 and Comparative Examples 4 and 5, it can be seen that heating treatment at 70-90°C during the grinding process can significantly improve its density, wear resistance and aging resistance. It is speculated that high temperature can promote the 3+ and Ce 4+ Solid solution into the zirconia lattice reduces the content of stabilizers at the grain boundaries. The increase in the chemical free enthalpy of the solid solution and the constraint energy between grains stabilizes the crystal form to remain in the tetragonal phase, reduces the volume expansion caused by the conversion of t-ZrO2→m-ZrO2 and causes micro cracks, and improves wear resistance. Most of the stabilizers in the composite stabilized zirconia prepared under low temperature conditions are at the grain boundaries, and are easily precipitated into the aqueous solution under low temperature aging conditions, resulting in phase change, thereby reducing wear resistance and having low anti-aging performance.

[0032] The wear resistance of zirconia grinding media is mainly determined by external and internal factors. When the external factors, i.e. the use conditions and environment, are determined, we can only improve the wear resistance from the internal factors. The internal factors mainly include phase, grain size, toughness, elastic modulus, strength, hardness and porosity (density). 3+ The presence of Ce makes it have higher strength and hardness. 4+ The presence of enhances its toughness and anti-aging performance, and it is not easy to crack due to phase change under long-term external force. The addition of kaolin as a sintering aid significantly reduces the sintering temperature, thereby reducing the grain size of the sintered body. The smaller grain size helps it maintain a stable tetragonal phase. High sintering activity promotes the densification process, accelerates the removal of pores, and reduces the presence of pores, thereby obtaining ultra-high density. Therefore, the cerium oxide and yttrium oxide composite stabilized zirconia grinding media has excellent comprehensive mechanical properties when sintered under low temperature conditions, thereby improving its wear resistance.

[0033] In summary, it can be concluded that the preparation method of a cerium oxide and yttria composite stabilized zirconia grinding medium of the present invention has an ultra-low sintering temperature of 1300-1350°C by adjusting the raw material ratio, controlling the sintering aid and the ball milling process. The prepared zirconia grinding medium has excellent low-temperature anti-aging performance and wear resistance, and its ultra-high density also helps it to be used in a high-viscosity grinding environment.

[0034] The present invention provides a cerium oxide / yttrium oxide composite stabilized zirconium oxide grinding medium and a preparation method thereof, wherein the preparation process is as follows: step 1, zirconium oxide, cerium oxide, yttrium oxide and kaolin are mixed, and then a dispersant and deionized water are added to grind to obtain a uniformly mixed slurry; step 2, the uniformly mixed slurry is subjected to centrifugal spray drying to obtain cerium oxide and yttrium oxide composite stabilized zirconium oxide powder; step 3, cerium oxide and yttrium oxide composite stabilized zirconium oxide powder are added to a binder for rolling molding to obtain a spherical grinding medium green body; step 4, the grinding medium green body is sintered and polished to obtain cerium oxide and yttrium oxide composite stabilized zirconium oxide grinding medium. Yttrium oxide and cerium oxide composite stabilized zirconium oxide are heat treated in a ball milling process, so that the tetragonal phase zirconium oxide can remain stable for a long time in a low temperature and humid environment, inhibit phase transition, have better anti-aging performance, and extend the service life. Wherein, by controlling the particle size, adding kaolin as a sintering aid, reducing the sintering temperature, using pressureless sintering, and sintering in an air atmosphere, high density can be obtained and cost can be reduced. The prepared grinding medium has excellent comprehensive mechanical properties, good wear resistance, low abrasion and reduced use cost.

[0035] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a cerium oxide / yttria composite stabilized zirconium oxide grinding medium, characterized in that: The following steps are included: Step 1: Mix zirconium oxide, cerium oxide, yttrium oxide and kaolin, add appropriate amount of dispersant and water to grind to obtain slurry, and keep the slurry temperature at 70-90°C during the grinding process; Step 2: centrifugal spray drying the slurry to obtain cerium oxide / yttria composite stabilized zirconium oxide powder; the spray drying atomizing disk speed is 9000-11000r / min, the inlet temperature is 240-260°C, and the outlet temperature is 95-110°C, so as to ensure that the granulated powder has good sphericity and fluidity; Step 3: adding the cerium oxide / yttria composite stabilized zirconium oxide powder to a binder and rolling-molding the powder to obtain a spherical grinding medium green body; Step 4: Sintering and polishing the green body of the spherical grinding medium to obtain a cerium oxide / yttria composite stabilized zirconium oxide grinding medium; In the step 1, the added amounts of zirconium oxide, cerium oxide, yttrium oxide and kaolin are 85-90wt%, 10-15wt%, 1-2wt% and 0.1-0.5wt%.

2. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding media according to claim 1, characterized in that: In the step 1, the added dispersant is Dolapix ce64, and the added amount is 0.5wt%.

3. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding media according to claim 1, characterized in that: In the step 1, the amount of water added is 50% and the solid content of the slurry is 50%.

4. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding medium according to claim 1, characterized in that: In the step 1, the mixed slurry grinding particle size D50 is controlled in the range of 0.15-0.2um.

5. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding media according to claim 1, characterized in that: In the step 2, the binder in the molding process is a mixture of PVA, glycerol and water.

6. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding media according to claim 1, characterized in that: In the step 4, the green body of the grinding medium is sintered by heating the temperature to 1300-1350° C. at a heating rate of 2° C. / min, keeping the temperature for 2-2.5 hours under pressureless conditions in an air atmosphere, and then naturally cooling to room temperature.

7. The method for preparing the cerium oxide / yttria composite stabilized zirconium oxide grinding media according to claim 1, characterized in that: In the step 4, the sintered grinding medium is polished by a sand mill at a line speed of 8 m / s, and the polishing material is white corundum with an addition amount of 2 wt%.

Citation Information

Patent Citations

  • Composite zirconium oxide nano-powder of cerium oxide / yttrium oxide and method of preparing the same

    CN101314542A

  • Ceramic and preparation method and application thereof

    CN102627457A

  • 3 YSZ nano powder, preparation method and use thereof

    CN106278255A

  • Rare-earth-doped zirconium oxide pressure transmitting medium as well as preparation method and application thereof

    CN118619693A

  • Zirconia porcelain and its production

    JP1992209761A

Cited By

  • Wear-resistant phase change energy storage material and preparation method thereof

    CN119592305A

  • Preparation process of anti-erosion high-purity zirconium oxide product

    CN119797909A

  • Alumina composite zirconia ceramic ball and preparation method thereof

    CN121974688A

  • An alumina-zirconia composite ceramic ball and its preparation method