Application of Ru-based perovskite catalyst in preparation of 1, 5-pentanediamine through decarboxylation of L-lysine

The ruthenium-containing perovskite oxide catalyst prepared by the sol-gel method is used in the selective decarboxylation reaction of L-lysine in high-temperature acid solution, which solves the problem of the catalyst's acid resistance and non-reduction resistance, and achieves high efficiency 1,5-pentanediamine selectivity and catalyst stability, the catalyst can be recycled multiple times.

CN119039151APending Publication Date: 2024-11-29EAST CHINA NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411204185.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the selectivity and catalyst stability of L-lysine decarboxylation are insufficient for preparing 1,5-pentanediamine, especially in high-temperature acid environments, the catalyst is not resistant to acid, does not resist reduction, and has a high loss rate, resulting in poor reaction selectivity. and poor cycle stability.

Method used

The sol-gel method is used to prepare a ruthenium-containing perovskite oxide catalyst, which is composed of ARuXB1-XO3, A is an alkaline earth metal element with a larger radius, and B is a transition metal separation element with a smaller radius, which is obtained by calcination and post-treatment. Catalyst for selective decarboxylation of L-lysine in high-temperature acidic solution.

Benefits of technology

The catalyst exhibits the characteristics of anti-reduction and acid etching in high-temperature acid solutions. It has low loss rate after multiple cycles, excellent catalytic performance, L-lysine conversion rate reaches 100%, and 1,5-pentanediamine selectivity ≥91%, and the catalyst can be recycled multiple times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to an application of a Ru-based perovskite catalyst in preparation of 1, 5-pentamethylene diamine through decarboxylation of L-lysine. The catalyst is composed of a ruthenium-containing perovskite oxide. The catalyst has the advantages that 1, the catalyst disclosed by the invention has the characteristics of reduction resistance and acid etching resistance in a high-temperature acid solution; and 2, the catalyst involved in the invention has excellent performance, the lysine conversion rate can reach 100%, the selectivity of the prepared 1, 5-pentanediamine is greater than or equal to 91%, and the catalyst can be recycled for multiple times and keeps high catalytic performance. And 3, the catalyst provided by the invention is simple in preparation method and convenient to recycle, and the product is easy to separate and can be recycled for multiple times. And 4, the bio-based L-lysine is used as the raw material, the raw material is cheap and easy to obtain, the reaction condition is mild, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing 1,5-pentanediamine by selective decarboxylation of L-lysine, and in particular to a method for preparing 1,5-pentanediamine by selective decarboxylation of L-lysine by using a Ru-based perovskite catalyst. Background Art

[0002] Nylon PA56 material can be produced by polymerization of 1,5-pentanediamine and adipic acid. It is a polyamide material that can be comparable to nylon 66 in performance and can be used as a substitute. As one of the polyester monomers for synthesizing nylon PA56, 1,5-pentanediamine is mainly produced by decarboxylation of L-lysine, which has a similar structure. In 2022, global lysine production reached about 3.86 million tons, and the price of lysine had dropped to about US$1.5 / kg in 2020. The use of L-lysine decarboxylation to prepare 1,5-pentanediamine not only helps solve the problem of overcapacity of L-lysine, but also drives the development of upstream and downstream industries of L-lysine. Limited by the existing inefficient production technology, the large-scale synthesis of 1,5-pentanediamine still faces huge challenges. Therefore, the development of efficient and green synthesis technology for bio-based 1,5-pentanediamine is the core of the production of nylon 56.

[0003] At present, L-lysine is mainly used to prepare 1,5-pentanediamine through bioenzyme catalysis, but the activity of lysine decarboxylase is inhibited by the concentration of substrate L-lysine and product 1,5-pentanediamine. In addition, during the decarboxylation of L-lysine to produce 1,5-pentanediamine, the pH of the reaction system continues to increase from acidic to alkaline, causing the enzyme to become unstable and unusable. The activity and stability issues of lysine decarboxylase limit the large-scale production of bioenzyme method.

[0004] Chemical decarboxylation is an efficient way to prepare 1,5-pentanediamine from L-lysine. Compared with the enzymes used in the biofermentation method, heterogeneous catalysts usually have good stability and are not affected by 1,5-pentanediamine. In particular, in the heterogeneous catalytic process, the product can be separated from the catalyst by simple centrifugation. In order to inhibit the growth of large-sized byproducts (lysinol, hydroxymethylpiperidine, etc.) mainly containing nitrogen heterocycles during the decarboxylation of lysine, it is of great significance to utilize the restriction effect of the carrier, such as hierarchical porous carbon materials or molecular sieves with rich channels. Verduyckt et al. used Ru / C catalyst. In acidic aqueous solution and 150°C, the conversion rate of L-lysine was 100%, the yield of 1,5-pentanediamine was 32%, and the yield of the byproduct lysinol reached 42%. Huang et al. developed a Mn-doped RuO2-Mn-Beta catalyst. Under the conditions of 200°C and 2MPaH2, the conversion rate of L-lysine was 100% and the selectivity of 1,5-pentanediamine was 54%. At present, the selectivity of chemical preparation of 1,5-pentanediamine is still very low, which is related to the unstable characteristics of the product 1,5-pentanediamine. In the presence of acidic sites and metals, 1,5-pentanediamine is easily deeply deaminated to form piperidine. In view of the difficulty of highly selective synthesis of 1,5-pentanediamine from L-lysine, the current focus of scientific research has been on developing a catalyst that has both high catalytic activity and can withstand high temperature acidic environments.

[0005] Perovskite, as a material with the same crystal structure, has excellent thermal and hydrothermal stability, as well as adjustable acidity and the ability to stabilize oxygen vacancies. The general formula is ABX3, where A is a larger cation occupying the edge of the unit cell, usually an alkaline earth or rare earth element, and B is a smaller transition metal cation coordinated with an anion X, generally an oxide, or nitride, halide, or sulfide. The perovskite structure can tolerate multiple substitutions of cation and anion sites, providing controllable oxygen and electron mobility, thermal stability, defects, and oxidation characteristics. It is often used as an efficient and stable heterogeneous catalyst to drive biorefining operations, including hydroprocessing, oxidation, steam reforming, and acid-base chemistry. The highly dispersed metals precipitated from perovskites can be used for hydrogenation and catalytic oxidation.

[0006] The redox properties of perovskites also promote the formation and stabilization of surface defects that can activate molecular oxygen or CO or CC bonds. Perovskites are thermally stable in inert or oxidizing environments and are easily doped at cationic or anionic sites to adjust vacancy formation, oxygen mobility and electronic conductivity, thereby adjusting the activity and selectivity of the catalyst. The purpose of the present disclosure is to provide a method for preparing a ruthenium-based perovskite catalyst and its application to solve the technical problems that ruthenium-based catalysts are not acid-resistant, not resistant to reduction, have high loss rates, and have poor selectivity for 1,5-pentanediamine and poor cyclic stability during the catalytic decarboxylation of lysine in aqueous solution. Summary of the invention

[0007] The reaction equation of the present invention is as follows:

[0008]

[0009] The catalyst has the characteristics of being resistant to reduction and acid etching in high-temperature acidic solutions, having low catalyst loss rate after multiple cycles, and having excellent catalyst performance. The catalyst can be recycled multiple times and maintain high catalytic performance, and the reaction conditions are mild and the process is simple.

[0010] To achieve the above objectives, the technical scheme adopted by the present invention is as follows: This scheme relates to the use of a ruthenium-containing perovskite oxide catalyst in the selective decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: the catalyst composition is ARu X B 1-X O3, wherein the A position is an alkaline earth metal element with a larger radius, such as Sr, Ba, etc.; the B position is a transition metal ion element with a smaller radius, such as Mn, Fe, Cu, etc. The ruthenium-containing perovskite oxide catalyst is prepared by a sol-gel method, and the specific implementation method is as follows:

[0011] Step 1, weigh 5.5-8 mmol A(OAc)2 into a beaker, where A is an alkaline earth metal ion with a larger radius, such as Sr 2 + , Ba 2+ Weigh 15-18mmol DL-malic acid, ruthenium acetate containing ammol of Ru, and B(NO3) containing (5-a)mmol of B. x In a beaker, B is a transition metal ion with a smaller radius, Mn 4+ , Fe 3+ , Cu 2+ One of them.

[0012] Step 2, add 50-80 mL of deionized water to the beaker and stir at room temperature for 1-3 hours.

[0013] Step 3, stirring and evaporating the solution at 343-373K, and drying the obtained sol at 443-523K for 30-60min to obtain a ruthenate catalyst precursor.

[0014] Step 4, calcining the ruthenate catalyst precursor at 823-1023K for 5-8h, and finally post-treating the calcined sample with 1-3M dilute nitric acid to remove residual ACO3.

[0015] Step 5, the catalyst prepared above is used for the decarboxylation of L-lysine to prepare 1,5-pentanediamine, and an aqueous solution of L-lysine, a catalyst, and a liquid acid are added to a high-pressure reactor, the pH of the solution is controlled within the range of 1-3, and the reactor is sealed. N2 is introduced to replace the air in the reactor, H2 is introduced into the reactor, the temperature of the reactor is raised to a specific temperature, and the reaction is carried out for a certain period of time to obtain a reaction solution. After the reaction is completed, H2 is released after the reactor is cooled, and the reaction solution is obtained by simply filtering the catalyst. Quantitative analysis is performed by liquid chromatography, and then the conversion rate of the reaction, the selectivity of the product, and the yield are calculated.

[0016] In the above method, the liquid acid is one or more combinations of sulfuric acid, hydrochloric acid, phosphoric acid, acetic acid, lactic acid, nitric acid, citric acid, and oxalic acid.

[0017] In the above method, the volume of the liquid acid is 5-1000uL.

[0018] In the above method, the concentration of the aqueous solution of L-lysine is 0.01-5 mol / L.

[0019] In the above method, the reaction temperature is 140-220° C., the hydrogen pressure is 0.5-3.0 MPa, and the reaction time is 1-5 h.

[0020] In summary, through the above method, the present invention has the following advantages and beneficial effects compared with the prior art:

[0021] 1. The catalyst involved in the present invention has the characteristics of being resistant to reduction and acid etching in high-temperature acidic solutions, and the loss rate of the catalyst after multiple cycles is ≤10%.

[0022] 2. The catalyst involved in the present invention has excellent performance, the lysine conversion rate can reach 100%, the selectivity of the prepared 1,5-pentanediamine is ≥91%, and the catalyst can be recycled for multiple times and maintain high catalytic performance.

[0023] 3. The catalyst preparation method involved in the present invention is simple, easy to recycle, the product is easy to separate, and can be recycled multiple times.

[0024] 4. The present invention uses cheap and readily available bio-based L-lysine as raw material, with mild reaction conditions and simple process. DETAILED DESCRIPTION

[0025] The instrument used for analyzing the composition of the liquid product is a Waters high performance liquid chromatograph, the chromatographic column is a C18 reverse phase column, the detector is an ultraviolet absorption detector, and the mobile phase is a mixed solution of 60% by volume acetonitrile and 40% by volume sodium acetate aqueous solution.

[0026]

[0027] Example 1

[0028] 5.5mmol Ba(OAc)2, 2.5mmol Ru(OAc) x , 2.5mmol Mn(NO3)2, 15.75mmol DL-malic acid were dissolved in 50mL water and stirred at room temperature for 2 hours. The solution was stirred and evaporated to dryness at 343K, and the obtained sol was dried at 463K for 30min to obtain a catalyst precursor. After the catalyst precursor was fully ground, it was placed in a muffle furnace and calcined at 823K for 5 hours to obtain BaRu 0.8 Mn 0.2 O3 and a small amount of BaCO3 mixture. Add 50mL of 0.1MHNO3 aqueous solution to the mixture powder and stir at room temperature for 30 minutes. Collect the resulting black precipitate by filtration, then wash with excess water and dry to obtain BaRu 0.5 Mn0.5O3 catalyst.

[0029] 0.3g of the prepared BaRu0.8Mn0.2O3 catalyst was added to the reactor, and 0.6g of lysine, 80ml of H2O, and 500uL of H3PO4 were added. The pH of the solution was 2.5. The reactor was sealed and H2 was introduced to replace the air in the reactor. 2MPa of H2 was introduced into the reactor, and the temperature of the reactor was raised to 180°C and the reaction was continued for 4h. After the reaction was completed, the reactor was cooled, H2 was released, and the reaction liquid was obtained by opening the reactor. Liquid chromatography was used for quantitative analysis. The product distribution is shown in Table 1.

[0030] Example 2

[0031] The operation is the same as in Example 1, except that 2.5 mmol Fe(NO3)3 is used instead of 2.5 mmol Mn(NO3)2. After calcination, the active catalyst BaRu provided by the present invention is obtained. 0.5 Fe 0.5 O3.

[0032] Example 3

[0033] The operation is the same as in Example 1, except that 2.5 mmol Cu(NO3)2 is used instead of 2.5 mmol Mn(NO3)2. After calcination, the active catalyst BaRu provided by the present invention is obtained. 0.5 Cu 0.5 O3.

[0034] Example 4

[0035] The operation was the same as in Example 1, except that 1 mmol Fe(NO3)3 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc)x Replace 2.5mmol Ru(OAc) x After calcination, the active catalyst BaRu provided by the present invention is obtained. 0.8 Fe 0.2 O3.

[0036] Example 5

[0037] The operation was the same as in Example 1, except that 1 mmol Cu(NO3)2 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc) x Replace 2.5mmol Ru(OAc) x After calcination, the active catalyst BaRu provided by the present invention is obtained. 0.8 Cu 0.2 O3.

[0038] Example 6

[0039] The operation was the same as in Example 1, except that 1 mmol Mn(NO3)2 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc) x Replace 2.5mmol Ru(OAc) x After calcination, the active catalyst BaRu provided by the present invention is obtained. 0.8 Mn 0.2 O3.

[0040] Example 7

[0041] The operation was the same as in Example 1, except that 5 mmol Ru(OAc) was used. x Substitution substitution 2.5mmol Ru(OAc) x Without adding 2.5 mmol Mn(NO3)z, the active catalyst BaRuO3 provided by the present invention is obtained after calcination.

[0042] Example 8

[0043] The operation was the same as in Example 1, except that 5.5 mmol Sr(OAc)2 was used instead of 5.5 mmol Ba(OAc)2. After calcination, the active catalyst SrRu provided by the present invention was obtained. 0.5 Mn0.5O3.

[0044] Example 9

[0045] The operation is the same as in Example 1, except that 2.5 mmol Fe(NO3)3 is substituted for 2.5 mmol Mn(NO3)2, and 5.5 mmol Sr(OAc)2 is substituted for 5.5 mmol Ba(OAc)2. After calcination, the active catalyst SrRu provided by the present invention is obtained. 0.5 Fe0.5 O3.

[0046] Example 10

[0047] The operation is the same as in Example 1, except that 2.5 mmol Cu(NO3)2 is substituted for 2.5 mmol Mn(NO3)2, and 5.5 mmol Sr(OAc)2 is substituted for 5.5 mmol Ba(OAc)2. After calcination, the active catalyst SrRu provided by the present invention is obtained. 0.5 Cu 0.5 O3.

[0048] Embodiment 11

[0049] The operation was the same as in Example 1, except that 1 mmol Fe(NO3)3 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc) x Replace 2.5mmol Ru(OAc) x , 5.5 mmol Sr(OAc)2 replaces 5.5 mmol Ba(OAc)2 and calcined to obtain the active catalyst SrRu provided by the present invention. 0.8 Fe 0.2 O3.

[0050] Example 12

[0051] The operation was the same as in Example 1, except that 1 mmol Cu(NO3)2 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc) x Replace 2.5mmol Ru(OAc) x , 5.5 mmol Sr(OAc)2 replaces 5.5 mmol Ba(OAc)2 and calcined to obtain the active catalyst SrRu provided by the present invention. 0.8 Cu 0.2 O3.

[0052] Embodiment 13

[0053] The operation was the same as in Example 1, except that 1 mmol Mn(NO3)2 was used instead of 2.5 mmol Mn(NO3)2 and 4 mmol Ru(OAc) x Replace 2.5mmol Ru(OAc) x , 5.5 mmol Sr(OAc)2 replaces 5.5 mmol Ba(OAc)2 and calcined to obtain the active catalyst SrRu provided by the present invention. 0.8 Mn 0.2 O3.

[0054] Embodiment 14

[0055] The operation was the same as in Example 1, except that 5 mmol Ru(OAc) was used. x Substitution substitution 2.5mmol Ru(OAc) x , 5.5 mmol Sr(OAc)2 replaces 5.5 mmol Ba(OAc)2, and 2.5 mmol Mn(NO3)2 is not added. After calcination, the active catalyst SrRuO3 provided by the present invention is obtained.

[0056] Table 1. Catalytic results of different ruthenium-based perovskite oxide catalysts for the decarboxylation of lysine to 1,5-pentanediamine

[0057]

[0058]

[0059] From the above results, it can be seen that the ruthenium-based perovskite oxide catalyst exhibits excellent catalytic performance in the selective decarboxylation of L-lysine to prepare 1,5-pentanediamine. The catalyst loss rate is low after multiple cycles, and the catalyst can be recycled many times and maintain high catalytic performance.

[0060] Embodiment 15

[0061] The operation was the same as in Example 1, except that HCl was used instead of H3PO4. The reaction results are shown in Table 2.

[0062] Example 16

[0063] The operation was the same as in Example 1, except that H2SO4 was used instead of H3PO4. The reaction results are shown in Table 2.

[0064] Embodiment 17

[0065] The operation was the same as in Example 1, except that HNO3 was used instead of H3PO4. The reaction results are shown in Table 2.

[0066] Embodiment 18

[0067] The operation was the same as in Example 1, except that CH3COOH was used instead of H3PO4. The reaction results are shown in Table 2.

[0068] Embodiment 19

[0069] The operation was the same as in Example 1, except that citric acid (C6H8O7) was used instead of H3PO4. The reaction results are shown in Table 2.

[0070] Embodiment 20

[0071] The operation was the same as in Example 1, except that H2C2O4 was used instead of H3PO4. The reaction results are shown in Table 2.

[0072] Embodiment 21

[0073] The operation was the same as in Example 1, except that lactic acid (C3H6O3) was used instead of H3PO4. The reaction results are shown in Table 2.

[0074] Table 2. Effects of different liquid acids on the selective decarboxylation of L-lysine to 1,5-pentanediamine

[0075]

[0076]

[0077] From the above results, it can be seen that the acidity of the liquid acid affects the selectivity of 1,5-pentanediamine. Strong acid will cause the acidity and alkalinity of the solution to fluctuate greatly, and the pH value of the solution cannot be controlled to remain constant; medium-strong acid will cause the acidity and alkalinity of the solution to fluctuate less, and the pH value can be controlled to remain within the range of 1-3; while weak acid will maintain the pH value of the solution at around 4-6, resulting in lower selectivity of pentamethylenediamine.

[0078] Embodiment 22

[0079] The reaction was carried out in a 300 ml high pressure reactor. 0.3 g of the prepared BaRu 0.8 Mn 0.2 O3 catalyst was added to the reactor, and 0.6g lysine, 80ml H2O, 500uL H3PO4 were added. The pH of the solution was 2.5. The reactor was sealed and H2 was introduced to replace the air in the reactor. 0.5-3MPa H2 was introduced into the reactor, and the temperature of the reactor was raised to 140-220°C and the reaction was carried out for 1-5h. After the reaction was completed, the reactor was cooled, H2 was released, and the reaction liquid was obtained. Liquid chromatography was used for quantitative analysis. The product distribution is shown in Table 3.

[0080] Table 3. Reaction performance of selective decarboxylation of L-lysine to 1,5.pentanediamine under different reaction conditions

[0081]

[0082]

[0083] From the results in Table 3, it can be seen that the reaction temperature, H2 pressure and reaction time have a great influence on the selective decarboxylation of L-lysine to prepare 1,5-pentanediamine. Increasing the temperature, increasing the H2 pressure and extending the reaction time are beneficial to the conversion of L-lysine, but too high a temperature, too high a H2 pressure and too long a reaction time will cause excessive aminolysis of 1,5-pentanediamine to generate by-products such as piperidine, resulting in an increase in by-products and ultimately a decrease in the selectivity of 1,5-pentanediamine. Therefore, appropriate temperature, H2 pressure and reaction time can control the decarboxylation reaction of L-lysine.

[0084] Embodiment 23

[0085] The operation was the same as in Example 1, except that the catalyst was recycled twice. The reaction results are shown in Table 4.

[0086] Embodiment 24

[0087] The operation was the same as in Example 1, except that the catalyst was circulated for reaction 3 times. The reaction results are shown in Table 4.

[0088] Embodiment 25

[0089] The operation was the same as in Example 1, except that the catalyst was circulated for 4 times. The reaction results are shown in Table 4.

[0090] Embodiment 26

[0091] The operation was the same as in Example 1, except that the catalyst was cyclically reacted 5 times. The reaction results are shown in Table 4.

[0092] Table 4 Stability test of ruthenium-based perovskite oxide catalysts

[0093]

[0094] The embodiments described above are only used to illustrate the technical ideas and features of the present invention, and their purpose is to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. The patent scope of the present invention cannot be limited only by these embodiments, that is, any equivalent changes or modifications made according to the spirit disclosed by the present invention still fall within the patent scope of the present invention.

Claims

1. Application of a Ru-based perovskite catalyst in the decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: The catalyst is a ruthenium-containing perovskite oxide with a general chemical formula of ARuxB1-xO3; the catalyst is a sparingly soluble ruthenate, wherein the A position is an alkaline earth metal element with a larger radius, such as Sr and Ba, and the B position is a transition metal ion element with a smaller radius, such as Mn, Fe, Cu, etc.

2. The use of the Ru-based perovskite catalyst according to claim 1 in the decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: The ruthenium-containing perovskite oxide catalyst is prepared by a sol-gel method, and the specific process is as follows: (a) weigh 5.5-8.0 mmol A(OAc)2 in a beaker, wherein A is an alkaline earth metal ion with a larger radius, such as Sr 2+ , Ba 2+ (b) weighing 15-18mmol DL-malic acid, ruthenium acetate containing ammol of Ru, and B (NO3) containing (5-a)mmol of B x in a beaker, where B is a transition metal ion with a smaller radius, such as Mn 4+ , Fe 3+ , Cu 2+ etc.; (c) adding 50-80 mL of deionized water to the beaker and stirring at room temperature for 1-3 h; (d) stirring and evaporating the solution at 343-373 K, and drying the obtained sol at 443-483 K for 30-60 min to obtain a ruthenate catalyst precursor; (e) calcining the ruthenate catalyst precursor at 823-1023 K for 5-8 h; (f) post-treating the calcined sample with 1-3 M dilute nitric acid to remove residual ACO3.

3. The use of the Ru-based perovskite catalyst according to claim 1 in the decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: The catalyst is used for selective decarboxylation of L-lysine to prepare 1,5-pentanediamine. In an aqueous solution of L-lysine, the concentration is 0.01-5 mol / L. Liquid acid is added to control the pH of the solution within the range of 1-3, a certain amount of catalyst is added, and the reaction is carried out under certain reaction temperature and hydrogen pressure conditions to decarboxylate and generate 1,5-pentanediamine in one step.

4. The use of the Ru-based perovskite catalyst according to claim 3 in the decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: The liquid acid is one or more combinations of sulfuric acid, hydrochloric acid, phosphoric acid, acetic acid, lactic acid, nitric acid, citric acid, and oxalic acid.

5. The use of the Ru-based perovskite catalyst according to claim 4 in the decarboxylation of L-lysine to prepare 1,5-pentanediamine, characterized in that: The reaction temperature is 140-220° C., the hydrogen pressure is 0.5-3.0 MPa, and the reaction time is 1-5 h.