Cable protective sleeve and production process thereof
By combining polyethylene resin and other materials and vulcanization processes, cross-linking networks and flame retardant systems are formed, the problems of poor tensile performance and insufficient flame retardant properties of cables are solved, and the flame retardant and tensile properties of cables are significantly improved, ensuring that The safety and reliability of robotic equipment.
Patent Information
- Application Number
- CN202411241816.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cables have poor tensile performance and insufficient flame retardancy during long-term use, which causes the robot equipment to fail to work normally and burn during fire, affecting use.
Use polyethylene resin, maleic anhydride grafted polyethylene, metallocene polyethylene, magnesium hydroxide, epoxy nanosilica, phosphobenzoxazine, silane-modified magnolia alcohol, antioxidants and promoters, etc. Materials, cable protective sleeves are prepared through plasticizing and vulcanizing processes to form a cross-linking network and flame retardant system to improve tensile and flame retardant performance.
Significantly improves the tensile performance and flame retardant effect of the cable, ensuring the safety and reliability of the cable under high temperature and fire conditions.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, in particular to a cable protective cover and a production process thereof. Background Art
[0002] Cable is a general term for items such as optical cables and electrical cables. Cables have many uses, mainly for controlling installation, connecting equipment, transmitting electricity and other multiple functions. For example, cables are widely used in the field of machinery and robot manufacturing. During long-term use, if the tensile performance is not good, the robot may not work normally. In the event of a fire, the low flame retardancy of the cables may cause them to burn, affecting the normal use of the robot. For example, patent CN116589778B announces an aging-resistant cable protective cover, a preparation method thereof and an aging-resistant cable. The cable of this invention improves the absorption effect of nano-titanium dioxide on ultraviolet rays and reduces the aging effect of ultraviolet rays on the protective cover, but its tensile and flame retardant effects are not improved. Summary of the invention
[0003] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a cable protective cover and a production process thereof, which has good flame retardant and tensile effects.
[0004] (II) Technical solution To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a cable protective cover, comprising the following components by weight: 40-60 parts by weight of polyethylene resin, 55-80 parts by weight of maleic anhydride grafted polyethylene, 35-50 parts by weight of metallocene polyethylene, 15-20 parts by weight of magnesium hydroxide, 10-15 parts by weight of epoxy nano-silica, 10-14 parts by weight of phosphorus-containing benzoxazine, 8-13 parts by weight of silane-modified magnolol, 1-2 parts by weight of antioxidant 1010, 0.3-0.5 parts by weight of vulcanizing agent DCP, and 0.2-0.6 parts by weight of accelerator TMTD.
[0005] Preferably, the preparation method of the phosphorus-containing benzoxazine is: (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and then drip phenylphosphonic acid dichloride into the reactor at room temperature for 18-22 minutes. After the dripping is completed, heat the mixture to 60-70°C and react for 8-12 hours. After the reaction is completed, wash with deionized water, and then distill to remove toluene to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, stir and mix, introduce nitrogen protection, heat to 65-80°C, stir and apply 360-400W / m 2UV irradiation, constant temperature stirring and irradiation reaction for 2-4 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, fully dissolving them, and carrying out a cyclization reaction at 70-90° C. for 12-16 hours. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-containing benzoxazine.
[0006] Preferably, the mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride in (1) is 1:0.01-0.03:1.1-1.3.
[0007] Preferably, the mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-mercaptopyrimidine and dimethylphenylphosphine catalyst in (2) is 0.8-1.2:1:0.02-0.04.
[0008] Preferably, the mass ratio of aminated magnolol, aqueous solution of formaldehyde and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol in (3) is 1:2.1-1.4:1.2-1.5.
[0009] Preferably, the preparation method of the silane-modified magnolol is: S1. Add 8-15 parts by weight of di(dimethylamino)methylvinylsilane and 10-12 parts by weight of phosphorus-modified magnolol to an acetonitrile solvent, stir to dissolve, then add 1-3 parts by weight of chloroplatinic acid catalyst, react at 65-80 ° C for 7-10h, and then rotary distill and wash to obtain an intermediate; S2. 4-9 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, 15-20 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 75-100°C for 4-8h. After the reaction, the reaction is carried out by reduced pressure distillation, washed and dried to obtain silane-modified magnolia alcohol.
[0010] The preferred preparation method of the cable protective cover is: polyethylene resin, maleic anhydride grafted polyethylene, metallocene polyethylene, magnesium hydroxide, epoxy nano-silica, phosphorus-containing benzoxazine, silane-modified magnolol, antioxidant 1010, added to a plasticizer, nitrogen protection, control the temperature to 40-60°C, the stirring rate to 30-45rpm, stirring and mixing for 30-50min to obtain a preliminary material; the preliminary material is transferred to an open mill, a vulcanizing agent DCP and an accelerator TMTD are added and mixed, extruded and shaped, and vulcanized. The barrel temperature of the extruder is set to: the temperature of zone 1 is 130°C, the temperature of zone 2 is 140°C, the temperature of zone 3 is 150°C, the temperature of zone 4 is 145°C, and the die head temperature is 155°C. After extrusion, it is placed in a flat vulcanizer, the vulcanization temperature is 180°C, and the vulcanization time is 10min to obtain a cable protective cover.
[0011] 3. Beneficial technical effects The invention provides a cable protective sleeve by adding polyethylene resin, maleic anhydride grafted polyethylene, metallocene polyethylene, magnesium hydroxide, epoxy nano-silica, phosphorus-containing benzoxazine, silane-modified magnolol and antioxidant 1010 into a plastic refiner, protecting with nitrogen, controlling temperature and stirring rate, stirring and mixing to obtain a primary material; transferring the primary material to an open mill, adding a vulcanizing agent DCP and an accelerator TMTD to mix, extruding to shape, and vulcanizing to form.
[0012] During the extrusion molding process, the hydroxyl groups in phosphorus-containing benzoxazine and silane-modified magnolia alcohol react with the epoxy groups in epoxy nano-silica and the anhydride groups in maleic anhydride-grafted polyethylene to form a cross-linked network, making the connection tighter and increasing its tensile properties. The phosphorus, silicon and sulfur elements contained in phosphorus-containing benzoxazine and silane-modified magnolia alcohol have good flame retardant effects, and the benzoxazine structure therein also has good flame retardant effects. In addition, the phosphorus-containing benzoxazine is a dibenzoxazine structure, which further improves its flame retardant effect and together constitutes a flame retardant system. DETAILED DESCRIPTION
[0013] Example 1 (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and drop phenylphosphonic acid dichloride into the reactor at room temperature, wherein the mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride is 1:0.01:1.1, and the dropping time is 18 minutes. After the dropping is completed, the temperature is raised to 60°C and reacted for 8 hours. After the end, the mixture is washed with deionized water, and then the toluene is removed by distillation to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, wherein the mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst is 0.8:1:0.02, stir and mix, introduce nitrogen protection, heat to 65°C, stir and assist with 360W / m 2 UV irradiation, constant temperature stirring and irradiation reaction for 2 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolia alcohol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, wherein the mass ratio of aminated magnolia alcohol, the aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol is 1:2.1:1.2, fully dissolving, and carrying out a cyclization reaction at 70°C for 12 hours. After completion, distilling under reduced pressure, washing with deionized water, and recrystallizing the crude product from dichloromethane to obtain phosphorus-containing benzoxazine; (4) Add 8 parts by weight of di(dimethylamino)methylvinylsilane and 10 parts by weight of phosphorus-modified magnolol to acetonitrile solvent, stir to dissolve, then add 1 part by weight of chloroplatinic acid catalyst, react at 65° C. for 7 h, and then perform rotary distillation and wash to obtain an intermediate; (5) 4 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, 15 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 75° C. for 4 hours. After the reaction is completed, the reaction is carried out by vacuum distillation, washing and drying to obtain silane-modified magnolol; (6) Add 40 parts by weight of polyethylene resin, 55 parts by weight of maleic anhydride grafted polyethylene, 35 parts by weight of metallocene polyethylene, 15 parts by weight of magnesium hydroxide, 10 parts by weight of epoxy nanosilica, 10 parts by weight of phosphorus-containing benzoxazine, 8 parts by weight of silane-modified magnolol, and 1 part by weight of antioxidant 1010 into a plasticizer, protect with nitrogen, control the temperature at 40°C, stir at a speed of 30 rpm, and stir and mix for 30 minutes to obtain a preliminary material; transfer the preliminary material to an open mixing mill, add 0.3 parts by weight of a vulcanizing agent DCP and 0.2 parts by weight of an accelerator TMTD, mix well, extrude and shape, and vulcanize to obtain a cable protective cover.
[0014] Example 2 (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and drop phenylphosphonic acid dichloride into the reactor at room temperature, wherein the mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride is 1: 0.03: 1.3, and the dropping time is 22 minutes. After the dropping is completed, the temperature is raised to 70°C and the reaction is carried out for 12 hours. After the end, the mixture is washed with deionized water, and then the toluene is removed by distillation to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, wherein the mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst is 1.2:1:0.04, stir and mix, introduce nitrogen protection, heat to 80°C, stir and supplement with 400W / m 2 UV irradiation, constant temperature stirring and irradiation reaction for 4 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolia alcohol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, wherein the mass ratio of aminated magnolia alcohol, the aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol is 1: 1.4:1.5, fully dissolving, and carrying out a cyclization reaction at 90° C. for 16 hours. After the reaction, distilling under reduced pressure, washing with deionized water, and recrystallizing the crude product from dichloromethane to obtain phosphorus-containing benzoxazine; (4) Add 15 parts by weight of di(dimethylamino)methylvinylsilane and 12 parts by weight of phosphorus-modified magnolol to an acetonitrile solvent, stir to dissolve, then add 3 parts by weight of chloroplatinic acid catalyst, react at 80° C. for 10 h, and then perform rotary distillation and wash to obtain an intermediate; (5) 9 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, 20 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 100° C. for 8 hours. After the reaction is completed, the mixture is distilled under reduced pressure, washed and dried to obtain silane-modified magnolol; (6) Add 60 parts by weight of polyethylene resin, 80 parts by weight of maleic anhydride grafted polyethylene, 50 parts by weight of metallocene polyethylene, 20 parts by weight of magnesium hydroxide, 15 parts by weight of epoxy nano-silica, 14 parts by weight of phosphorus-containing benzoxazine, 13 parts by weight of silane-modified magnolol, and 2 parts by weight of antioxidant 1010 into a plasticizer, protect with nitrogen, control the temperature at 60°C, stir at 45 rpm, and stir and mix for 50 minutes to obtain a preliminary material; transfer the preliminary material to an open mixing mill, add 0.5 parts by weight of a vulcanizing agent DCP and 0.6 parts by weight of an accelerator TMTD, mix well, extrude and shape, and vulcanize to obtain a cable protective cover.
[0015] Example 3 (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and drop phenylphosphonic acid dichloride into the reactor at room temperature, wherein the mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride is 1:0.02:1.2, and the dropping time is 20 minutes. After the dropping is completed, the temperature is raised to 65°C and reacted for 10 hours. After the end, the mixture is washed with deionized water, and then the toluene is removed by distillation to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, wherein the mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst is 1:1:0.03, stir and mix, introduce nitrogen protection, heat to 72°C, stir and assist with 380W / m 2 UV irradiation, constant temperature stirring and irradiation reaction for 3 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolia alcohol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, wherein the mass ratio of aminated magnolia alcohol, the aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol is 1:2.2:1.3, fully dissolving, and carrying out a cyclization reaction at 80°C for 14 hours. After completion, the reaction is distilled under reduced pressure, washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain phosphorus-containing benzoxazine; (4) Add 11 parts by weight of di(dimethylamino)methylvinylsilane and 11 parts by weight of phosphorus-modified magnolol to acetonitrile solvent, stir to dissolve, then add 2 parts by weight of chloroplatinic acid catalyst, react at 72° C. for 8 h, and then perform rotary distillation and wash to obtain an intermediate; (5) 6 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, and 17 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 87° C. for 6 hours. After the reaction is completed, the reaction is carried out by vacuum distillation, washing and drying to obtain silane-modified magnolol; (6) Add 50 parts by weight of polyethylene resin, 65 parts by weight of maleic anhydride grafted polyethylene, 42 parts by weight of metallocene polyethylene, 17 parts by weight of magnesium hydroxide, 12 parts by weight of epoxy nano-silica, 12 parts by weight of phosphorus-containing benzoxazine, 11 parts by weight of silane-modified magnolol, and 1.5 parts by weight of antioxidant 1010 into a plasticizer, protect with nitrogen, control the temperature at 50°C, stir at a speed of 37 rpm, and stir and mix for 40 minutes to obtain a preliminary material; transfer the preliminary material to an open mixing mill, add 0.4 parts by weight of a vulcanizing agent DCP and 0.4 parts by weight of an accelerator TMTD, mix well, extrude and shape, and vulcanize to obtain a cable protective cover.
[0016] Example 4 (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and drop phenylphosphonic acid dichloride into the reactor at room temperature, wherein the mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride is 1:0.01:1.1, and the dropping time is 18 minutes. After the dropping is completed, the temperature is raised to 60°C and reacted for 8 hours. After the end, the mixture is washed with deionized water, and then the toluene is removed by distillation to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, wherein the mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst is 0.8:1:0.02, stir and mix, introduce nitrogen protection, heat to 65°C, stir and assist with 360W / m 2 UV irradiation, constant temperature stirring and irradiation reaction for 2 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolia alcohol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, wherein the mass ratio of aminated magnolia alcohol, the aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol is 1: 1.4:1.5, fully dissolving, and carrying out a cyclization reaction at 90° C. for 16 hours. After the reaction, distilling under reduced pressure, washing with deionized water, and recrystallizing the crude product from dichloromethane to obtain phosphorus-containing benzoxazine; (4) Add 15 parts by weight of di(dimethylamino)methylvinylsilane and 12 parts by weight of phosphorus-modified magnolol to an acetonitrile solvent, stir to dissolve, then add 3 parts by weight of chloroplatinic acid catalyst, react at 80° C. for 10 h, and then perform rotary distillation and wash to obtain an intermediate; (5) 6 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, and 17 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 87° C. for 6 hours. After the reaction is completed, the reaction is carried out by vacuum distillation, washing and drying to obtain silane-modified magnolol; (6) Add 50 parts by weight of polyethylene resin, 65 parts by weight of maleic anhydride grafted polyethylene, 42 parts by weight of metallocene polyethylene, 17 parts by weight of magnesium hydroxide, 12 parts by weight of epoxy nano-silica, 12 parts by weight of phosphorus-containing benzoxazine, 11 parts by weight of silane-modified magnolol, and 1.5 parts by weight of antioxidant 1010 into a plasticizer, protect with nitrogen, control the temperature at 50°C, stir at a speed of 37 rpm, and stir and mix for 40 minutes to obtain a preliminary material; transfer the preliminary material to an open mixing mill, add 0.4 parts by weight of a vulcanizing agent DCP and 0.4 parts by weight of an accelerator TMTD, mix well, extrude and shape, and vulcanize to obtain a cable protective cover.
[0017] Comparative Example 1 (1) 50 parts by weight of polyethylene resin, 65 parts by weight of maleic anhydride grafted polyethylene, 42 parts by weight of metallocene polyethylene, 17 parts by weight of magnesium hydroxide, 12 parts by weight of epoxy nano-silica, 11 parts by weight of silane-modified magnolol, and 1.5 parts by weight of antioxidant 1010 are added to a plasticizer, and the temperature is controlled at 50° C. and the stirring rate is 37 rpm under nitrogen protection. The mixture is stirred and mixed for 40 minutes to obtain a preliminary material. The preliminary material is transferred to an open mixing mill, 0.4 parts by weight of a vulcanizing agent DCP and 0.4 parts by weight of an accelerator TMTD are added and mixed, and the mixture is extruded, shaped, and vulcanized to obtain a cable protective sleeve.
[0018] Comparative Example 2 (1) 50 parts by weight of polyethylene resin, 65 parts by weight of maleic anhydride grafted polyethylene, 42 parts by weight of metallocene polyethylene, 17 parts by weight of magnesium hydroxide, 12 parts by weight of epoxy nano-silica, 12 parts by weight of phosphorus-containing benzoxazine, and 1.5 parts by weight of antioxidant 1010 are added to a plasticizer, and the temperature is controlled at 50°C and the stirring rate is 37 rpm under nitrogen protection. The mixture is stirred and mixed for 40 minutes to obtain a primary material. The primary material is transferred to an open mixing mill, 0.4 parts by weight of a vulcanizing agent DCP and 0.4 parts by weight of an accelerator TMTD are added and mixed, and the mixture is extruded, shaped, and vulcanized to obtain a cable protective sleeve.
[0019] Use an oxygen index meter to test the limiting oxygen index of water-based paint; use a horizontal and vertical combustion instrument to test the combustion level of water-based paint.
[0020] Table 1: Flame retardancy tests.
[0021] project Limiting oxygen index (%) Combustion level Example 1 31 V-0 Example 2 33 V-0 Example 3 31 V-0 Example 4 32 V-0 Comparative Example 1 21 V-1 Comparative Example 2 22 V-1 It can be seen from Table 1 that the flame retardant effect of Examples 1-4 is better than that of Comparative Examples 1-2, which indicates that the cable protective cover prepared by the present invention has good flame retardant effect.
[0022] The tensile test was carried out in accordance with GB / T 1040.1-2018. The test results are shown in Table 2.
[0023] Table 2: Tensile strength test.
[0024] project Tensile strength (MPa) Example 1 55.4 Example 2 56.7 Example 3 55.9 Example 4 54.7 Comparative Example 1 28.3 Comparative Example 2 29.5 It can be seen from Table 2 that the cable protective cover embodiments 1-4 of the present invention have better tensile properties than the comparative examples 1-2.
[0025] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A cable protective cover, characterized in that: The invention comprises the following components by weight: 40-60 parts by weight of polyethylene resin, 55-80 parts by weight of maleic anhydride grafted polyethylene, 35-50 parts by weight of metallocene polyethylene, 15-20 parts by weight of magnesium hydroxide, 10-15 parts by weight of epoxy nano-silica, 10-14 parts by weight of phosphorus-containing benzoxazine, 8-13 parts by weight of silane-modified magnolol, 1-2 parts by weight of antioxidant 1010, 0.3-0.5 parts by weight of vulcanizing agent DCP and 0.2-0.6 parts by weight of accelerator TMTD.
2. The cable protective cover according to claim 1, characterized in that: The preparation method of the phosphorus-containing benzoxazine is: (1) Add magnolol and triethylamine into a reactor containing toluene solvent, stir and mix, and then drip phenylphosphonic acid dichloride into the reactor at room temperature for 18-22 minutes. After the dripping is completed, heat the mixture to 60-70°C and react for 8-12 hours. After the reaction is completed, wash with deionized water, and then distill to remove toluene to obtain phosphorus-modified magnolol; (2) Add phosphorus-modified magnolol, 4,6-diamino-2-thiopyrimidine and dimethylphenylphosphine catalyst to dimethyl sulfoxide solvent, stir and mix, introduce nitrogen protection, heat to 65-80°C, stir and apply 360-400W / m 2 UV irradiation, constant temperature stirring and irradiation reaction for 2-4 hours, after the reaction is completed, the solvent is removed by vacuum rotary evaporation to obtain aminated magnolol; (3) Adding aminated magnolol, an aqueous solution of formaldehyde, and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol to a toluene solvent, fully dissolving them, and carrying out a cyclization reaction at 70-90° C. for 12-16 hours. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-containing benzoxazine.
3. The cable protective cover according to claim 2, characterized in that: The mass ratio of magnolol, triethylamine and phenylphosphonic acid dichloride in (1) is 1:0.01-0.03:1.1-1.
3.
4. The cable protective cover according to claim 2, characterized in that: The mass ratio of phosphorus-modified magnolol, 4,6-diamino-2-mercaptopyrimidine and dimethylphenylphosphine catalyst in (2) is 0.8-1.2:1:0.02-0.
04.
5. The cable protective cover according to claim 2, characterized in that: The mass ratio of aminated magnolol, aqueous solution of formaldehyde and 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol in (3) is 1:2.1-1.4:1.2-1.
5.
6. The cable protective cover according to claim 1, characterized in that: The preparation method of the silane-modified magnolia alcohol is: S1. Add 8-15 parts by weight of di(dimethylamino)methylvinylsilane and 10-12 parts by weight of phosphorus-modified magnolol to an acetonitrile solvent, stir to dissolve, then add 1-3 parts by weight of chloroplatinic acid catalyst, react at 65-80 ° C for 7-10h, and then rotary distill and wash to obtain an intermediate; S2. 4-9 parts by weight of the intermediate is added to N,N-dimethylformamide solvent, stirred evenly, 15-20 parts by weight of chloroethanol is added thereto, and the reaction is carried out at 75-100°C for 4-8h. After the reaction, the reaction is carried out by reduced pressure distillation, washed and dried to obtain silane-modified magnolia alcohol.
7. A method for preparing a cable protective cover according to any one of claims 1 to 6, characterized in that: The preparation method of the cable protective cover comprises the following steps: adding polyethylene resin, maleic anhydride grafted polyethylene, metallocene polyethylene, magnesium hydroxide, epoxy nano-silica, phosphorus-containing benzoxazine, silane-modified magnolol, and antioxidant 1010 into a plasticizer, protecting with nitrogen, controlling the temperature to 40-60° C., stirring at a speed of 30-45 rpm, stirring and mixing for 30-50 minutes to obtain a primary material; transferring the primary material into an open mill, adding a vulcanizing agent DCP and an accelerator TMTD to mix, extruding and shaping, and vulcanizing to obtain the cable protective cover.