Low-temperature rapidly vulcanized liquid silicone rubber and preparation process thereof

By using a low-temperature, rapid vulcanization liquid silicone rubber with specific components and processes, the problem of premature vulcanization caused by improper operation time has been solved, achieving low-temperature rapid vulcanization and efficient production, thereby improving product quality and performance.

CN119039792AInactive Publication Date: 2024-11-29东莞市万觅新材料科技有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411378821.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing low-temperature rapid vulcanization liquid silicone rubber production process, improper operation time can easily lead to premature vulcanization or incomplete vulcanization of the material, affecting production efficiency and product quality.

Method used

By using a specific ratio of vinyl-terminated polydimethylsiloxane, reinforcing filler, molecular structure control agent, hydrogen-containing silicone oil, catalyst and inhibitor, and through segmented mixing and step-by-step stirring processes, the vulcanization reaction time and rate are controlled to ensure that the material vulcanizes rapidly at low temperatures.

Benefits of technology

This technology enables rapid vulcanization at low temperatures, improving production efficiency, ensuring sufficient processing time for materials, and enhancing product quality and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039792A_ABST
    Figure CN119039792A_ABST
Patent Text Reader

Abstract

The invention discloses low-temperature rapidly vulcanized liquid silicone rubber and a preparation process thereof. The low-temperature rapidly vulcanized liquid silicone rubber is prepared from the following components in percentage by mass: 60%-70% of vinyl-terminated polydimethylsiloxane, 17%-20% of reinforcing filler, 13%-20% of a molecular structure control agent, 2%-4% of hydrogen-containing silicone oil, 0.1%-0.2% of a catalyst and 0.03%-0.05% of an inhibitor. Then respectively adding vinyl-terminated polydimethylsiloxane, a reinforcing filler and a molecular structure control agent into a kneading machine, and uniformly stirring at room temperature; after stirring is completed, the materials are put into a kneading machine to be subjected to high-temperature refining in a vacuum environment, and base rubber is formed; the preparation method comprises the following steps: uniformly dividing basic glue into two parts, adding a catalyst into one part, and uniformly stirring at room temperature to form glue A; adding hydrogen-containing silicone oil and a catalyst into the other part, and uniformly stirring at room temperature to form glue B; and mixing the glue A and the glue B, stirring and vulcanizing to form a finished product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a liquid silicone rubber and a preparation method thereof, and in particular to a low-temperature fast-vulcanizing liquid silicone rubber and a preparation process thereof. Background Art

[0002] Low-temperature fast-vulcanizing liquid silicone rubber is a silicone rubber material that can quickly complete the vulcanization process at a relatively low temperature. Since the vulcanization reaction can be carried out at a lower temperature, compared with traditional high-temperature vulcanized silicone rubber, it can greatly reduce energy consumption and the risk of thermal damage to the packaged material. For example, in the packaging of electronic components, low-temperature vulcanization can avoid damage to sensitive electronic components caused by high temperatures.

[0003] In the existing production process of low-temperature rapid vulcanization liquid silicone rubber, multiple operation links such as mixing and molding are required. If the material reaction is too short, the operation time will be too short, and workers may not have enough time to complete various operations, affecting production efficiency and product quality. If the material reaction is too long, the operation time will be too long, and the silicone rubber may be vulcanized prematurely during the operation, causing the material to become viscous or even solidified, making it impossible to perform subsequent molding and other operations. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a low-temperature fast-vulcanizing liquid silicone rubber, according to the following components in percentage by mass: 60%-70% of terminal vinyl polydimethylsiloxane, 17%-20% of reinforcing filler, 13%-20% of molecular structure controller, 2%-4% of hydrogen-containing silicone oil, 0.1%-0.2% of catalyst and 0.03%-0.05% of inhibitor.

[0005] Furthermore, the vinyl-terminated polydimethylsiloxane contains vinyl groups with a content of 0.15-0.5 mol %, and the reinforcing filler is fumed silica with a specific surface area of ​​150-380 m2 / g.

[0006] Furthermore, the molecular structure control agent is one or a combination of two of hydroxyl-containing silane, alkoxy silane, silazane and boron-containing siloxane.

[0007] Furthermore, the catalyst is a platinum catalyst.

[0008] Furthermore, the inhibitor is one or a combination of two of ethynyl cyclohexanol, methyl butynol and diethyl maleate.

[0009] Furthermore, the hydroxyl-containing silane is methyltrihydroxysilane, the alkoxysilane is methyltrimethoxysilane or vinyltrimethoxysilane, the silazane is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and the boron-containing siloxane is a high molecular weight linear boron siloxane polymer.

[0010] The present application also provides a process for preparing low-temperature fast-vulcanizing liquid silicone rubber, comprising the following steps: Step 1: Add terminal vinyl polydimethylsiloxane, reinforcing filler and molecular structure control agent into a kneader respectively and stir evenly at room temperature; Step 2: After stirring, put the above materials into a kneader under vacuum environment for refining to form a base rubber; Step 3: Divide the base rubber into two parts, add a catalyst to one part, stir evenly at room temperature to form A rubber; add hydrogen-containing silicone oil and a catalyst to the other part, stir evenly at room temperature to form B rubber; Step 4: Mix A rubber and B rubber together, stir and vulcanize to form a finished product.

[0011] Furthermore, in the step 1, the stirring time at room temperature is 1.5-2 hours.

[0012] Furthermore, in the step 2, the temperature in the vacuum environment is 160°C-180°C, and the refining time is 2 hours.

[0013] Compared with the prior art, the present invention has the following beneficial effects: 1. The present application can affect the molecular chain structure of silicone rubber by adding a molecular structure control agent, so that it has a more suitable viscosity and fluidity before vulcanization. The molecular structure control agent can interact with silicone rubber molecules, increase the distance between molecules, reduce viscosity, and thus control the operation time. The appropriate molecular chain structure can make the material easier to operate during processing, and also help improve the quality and performance of the product. At the same time, it can interact with the catalyst or cross-linking agent in the vulcanization system to reduce their activity, thereby delaying the vulcanization reaction.

[0014] 2. In addition, the present application adopts a segmented mixing method, firstly mixing part of the additives with the vinyl-terminated polydimethylsiloxane, and then adding the remaining additives for thorough mixing. This can avoid the problem of long mixing time or uneven mixing caused by adding all the additives at once, and can also extend the operation time.

[0015] Additional aspects and advantages of the present invention will be given in part in the description which follows, and in part will be obvious from the description which follows, or may be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0017] Figure 1 It is a schematic diagram of the preparation process of the present invention; DETAILED DESCRIPTION The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The present invention is described in more detail. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. It should be noted that when an element is described as "fixed to" another element, it can be directly on the other element, or there can be one or more centered elements therebetween. When an element is described as "connected to" another element, it can be directly connected to the other element, or there can be one or more centered elements therebetween.

[0019] In the description of the present invention, it should be noted that the orientation or positional relationship indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, vertical, horizontal" and "top, bottom" are usually based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description. Unless otherwise stated, these directional words do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present invention; the directional words "inside and outside" refer to the inside and outside relative to the outline of each component itself. In the description of the present invention, it should be noted that the use of words such as "first" and "second" to define components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above words have no special meaning, and therefore cannot be understood as limiting the scope of protection of the present invention. In the description of the embodiments of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0020] The present application provides a low-temperature, fast-vulcanizing liquid silicone rubber, a first embodiment of which is as follows: the components are arranged in the following mass percentages: 60% of vinyl-terminated polydimethylsiloxane, 17% of reinforcing filler, 13% of molecular structure controller, 4% of hydrogenated silicone oil, 0.2% of catalyst and 0.05% of inhibitor.

[0021] The reinforcing filler used for reinforcing fillers can form physical or chemical bonds with silicone rubber molecules, increase the crosslinking density of silicone rubber, and thus significantly improve the mechanical properties of silicone rubber such as tensile strength, tear strength and tensile strength. At the same time, the reinforcing filler can also reduce the friction coefficient of silicone rubber, reduce the heat generated by friction, and improve the wear resistance and heat resistance of silicone rubber; the molecular structure controller is used to affect the molecular chain structure of silicone rubber so that it has a more suitable viscosity and fluidity before vulcanization. The molecular structure controller can interact with silicone rubber molecules, increase the distance between molecules, reduce viscosity, and thus control the operation time. A suitable molecular chain structure can make the material easier to operate during processing, and also help to improve the quality and performance of the product. At the same time, it can react with the catalyst or crosslinker in the vulcanization system to reduce their activity, thereby delaying the vulcanization reaction; the silicon-hydrogen bond (Si-H) of the hydrogen-containing silicone oil reacts with active groups such as vinyl in silicone rubber under the action of a catalyst (such as a platinum catalyst) to form a crosslinked structure, thereby converting the silicone rubber from a plastic state to a vulcanized state with a certain strength and elasticity. This cross-linking reaction can be carried out quickly at a relatively low temperature, thus achieving low-temperature rapid vulcanization of silicone rubber. For example, at a temperature of 80-120°C, hydrogen-containing silicone oil can undergo an effective vulcanization reaction with silicone rubber, greatly reducing the temperature and time required for vulcanization; the catalyst and inhibitor are used to control the time and rate of the entire material reaction.

[0022] On the basis of the above embodiment, the vinyl-terminated polydimethylsiloxane contains vinyl, and the vinyl has a high reactivity during the vulcanization process. In the low-temperature rapid vulcanization liquid silicone rubber system, the vinyl can react rapidly with cross-linking agents such as hydrogenated silicone oil under the action of a catalyst to form a cross-linked network structure, so that the silicone rubber can quickly complete vulcanization at a lower temperature, greatly improving production efficiency. This is not only conducive to the uniform dispersion of fillers in silicone rubber, but also can improve the reinforcing effect of fillers, so that the performance of silicone rubber can be more fully utilized. Preferably, the vinyl-terminated polydimethylsiloxane contains vinyl, and the content is 0.15-0.5mol%.

[0023] Further on the basis of the above embodiment, the reinforcing filler is fumed silica, which can form physical or chemical bonds with silicone rubber molecules, increase the crosslinking density of silicone rubber, and thus significantly improve the mechanical properties of silicone rubber such as tensile strength, tear strength and tensile strength. Its fine particle size and high specific surface area enable it to fully contact with silicone rubber molecules, effectively transfer stress, and prevent the expansion of cracks. At the same time, fumed silica has a very high specific surface area, usually between 50-400 square meters / gram. The high specific surface area enables silica to fully contact with silicone rubber molecules, providing more binding sites, thereby enhancing the reinforcing effect. Compared with other reinforcing fillers, fumed silica can achieve better mechanical performance improvement at a lower dosage. Preferably, the specific surface area of ​​the fumed silica is between 150-380 square meters / gram.

[0024] On the basis of the above-mentioned embodiment, the molecular structure control agent is one or a combination of two of hydroxy-containing silane, alkoxysilane, silazane and boron-containing siloxane. The effect of the above-mentioned molecular structure control agent is to better react the vinyl-terminated polydimethylsiloxane with the catalyst, so as to control the reaction time and reaction rate. Specifically, the hydroxy-containing silane can react with the catalyst in the vulcanization system to cross-link, thereby delaying the start of the vulcanization reaction. This allows more time to carry out operations such as banburying and molding during processing, avoiding the problem of premature curing of materials due to too fast vulcanization, and being unable to carry out subsequent processing. Meanwhile, by adjusting the amount of hydroxy-containing silane, the speed of the vulcanization reaction can be controlled. An appropriate amount of hydroxy-containing silane can make the vulcanization reaction proceed at a suitable speed at low temperatures, which not only ensures the requirement of rapid vulcanization, but also does not affect the product quality too fast. Preferably, the hydroxy-containing silane can be methyltrihydroxysilane.

[0025] The alkoxysilane can react with the components in the vulcanization system to delay the start of the vulcanization reaction. This is very important for the low-temperature rapid vulcanization process, which can prevent the silicone rubber from vulcanizing prematurely during processing, ensure that there is enough time for operations such as mixing and molding, and improve production efficiency and product quality. At the same time, by adjusting the dosage and type of alkoxysilane, the speed of the vulcanization reaction can be controlled so that it can be carried out quickly and appropriately at low temperatures. It can not only meet the requirements of rapid vulcanization, but also avoid product defects or unstable performance caused by too fast a vulcanization speed. Preferably, the alkoxysilane is methyltrimethoxysilane or vinyltrimethoxysilane.

[0026] Since there are a large number of hydroxyl groups on the surface of white carbon black, these hydroxyl groups will physically or chemically adsorb with silicone rubber molecules, causing the rubber to gradually harden and reduce plasticity during processing and storage, resulting in structural phenomena. The role of the silazane is that the active groups in the silazane can preferentially react with the hydroxyl groups on the surface of white carbon black to passivate the hydroxyl groups, thereby inhibiting the generation of structuralization and maintaining the processing performance and plasticity of silicone rubber. Preferably, the silazane is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane.

[0027] The boron-containing siloxane can reduce the vulcanization temperature of silicone rubber. Boron atoms have a high electron cloud density and can form a strong interaction with other atoms in silicone rubber molecules, thereby reducing the energy required for the vulcanization reaction. This allows silicone rubber to be vulcanized at a lower temperature, reducing energy consumption and also reducing the requirements for equipment and processes. Preferably, the boron-containing siloxane is a high molecular weight linear borosiloxane polymer.

[0028] Further on the basis of the above embodiment, the catalyst is a platinum catalyst, which can greatly accelerate the vulcanization reaction of silicone rubber under low temperature conditions. Compared with traditional catalysts, it can trigger a cross-linking reaction at a lower temperature, so that silicone rubber can complete the vulcanization process in a shorter time. For example, at a temperature of 80-120°C, a platinum catalyst can promote rapid vulcanization of silicone rubber, while other catalysts may require higher temperatures to achieve similar reaction rates. This efficient catalytic effect can significantly improve production efficiency, reduce energy consumption, and also reduce the risk of thermal damage to the vulcanized material. Especially for some temperature-sensitive application fields, such as electronic component packaging, medical equipment manufacturing, etc., low-temperature rapid vulcanization is particularly important.

[0029] On the basis of the above-described embodiment, the inhibitor is a combination of one or two of ethynyl cyclohexanol, methyl butynol and diethyl maleate, and the effect of the inhibitor is to effectively delay the start of the vulcanization reaction in the low temperature rapid vulcanization liquid silicone rubber system. This is very critical for the actual production process, because in the processing and molding stage, a certain amount of time is required to carry out operations such as mixing, extrusion, injection molding. If the vulcanization reaction is started too early, the material will be cured too early in the processing equipment, affecting the continuity of production and product quality. By inhibiting the start of the vulcanization reaction, the inhibitor provides a suitable operating time window for the operator. Within this time range, various processing operations can be performed on silicone rubber, such as adjusting the formula, adding fillers, changing the color, etc. This can better meet the production needs of different products and improve the flexibility and controllability of production.

[0030] The present application provides a second embodiment, which is different from the first embodiment in that the components are in the following mass percentages: 70% of terminal vinyl polydimethylsiloxane, 20% of reinforcing filler, 20% of molecular structure control agent, 2% of hydrogen-containing silicone oil, 0.1% of catalyst and 0.03% of inhibitor.

[0031] The present application also provides a process for preparing low temperature fast vulcanized liquid silicone rubber, such as Figure 1 As shown, it includes the following steps: step 1: adding terminal vinyl polydimethylsiloxane, reinforcing filler and molecular structure control agent into a kneader respectively and stirring them evenly at room temperature; step 2: after stirring, putting the above materials into a kneader under a vacuum environment for refining to form a base rubber; step 3, dividing the base rubber into two parts, adding a catalyst into one part, stirring evenly at room temperature to form A rubber; adding hydrogen-containing silicone oil and a catalyst into the other part, stirring evenly at room temperature to form B rubber; step 4: mixing A rubber and B rubber together, stirring and vulcanizing to form a finished product.

[0032] From the above examples, it can be seen that part of the additives are firstly kneaded with the vinyl-terminated polydimethylsiloxane to form a base rubber, and then the base rubber is evenly divided, and then evenly divided into two parts, and different remaining additives are added to each part, and then fully stirred. This can avoid the problem of long or uneven kneading time caused by adding all the additives at one time, and can also control and delay the operation time.

[0033] Further to the above embodiment, in step 1, the stirring time at room temperature is 1.5-2 hours, so that more sufficient stirring can be achieved.

[0034] Further on the basis of the above embodiment, in the step 2, the temperature in the vacuum environment is 160°C-180°C, and the refining time is 2 hours.

[0035] The details of the exemplary embodiments described above are not limited to the embodiments described above, and the invention may be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive in all respects, and the scope of the invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the invention.

Claims

1. A low temperature fast vulcanizing liquid silicone rubber, It is characterized in that The components are arranged in the following mass percentages: 60%-70% of vinyl-terminated polydimethylsiloxane, 17%-20% of reinforcing filler, 13%-20% of molecular structure controller, 2%-4% of hydrogen-containing silicone oil, 0.1%-0.2% of catalyst and 0.03%-0.05% of inhibitor.

2. The low-temperature fast-vulcanizing liquid silicone rubber according to claim 1, It is characterized in that The vinyl-terminated polydimethylsiloxane contains vinyl groups with a content of 0.15-0.5 mol %. The reinforcing filler is fumed silica with a specific surface area of ​​150-380 m2 / g.

3. The low-temperature fast-vulcanizing liquid silicone rubber according to claim 1, It is characterized in that The molecular structure control agent is one or a combination of two of hydroxyl-containing silane, alkoxy silane, silazane and boron-containing siloxane.

4. The low-temperature fast-vulcanizing liquid silicone rubber according to claim 1, It is characterized in that The catalyst is a platinum catalyst.

5. The low-temperature fast-vulcanizing liquid silicone rubber according to claim 1, It is characterized in that The inhibitor is one or a combination of two of ethynyl cyclohexanol, methyl butynol and diethyl maleate.

6. The low-temperature fast-vulcanizing liquid silicone rubber according to claim 3, It is characterized in that The hydroxyl-containing silane is methyltrihydroxysilane, the alkoxysilane is methyltrimethoxysilane or vinyltrimethoxysilane, the silazane is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and the boron-containing siloxane is a high molecular weight linear boron siloxane polymer.

7. A process for preparing low-temperature fast-vulcanizing liquid silicone rubber, It is characterized in that The following steps are included: Step 1: Add the vinyl-terminated polydimethylsiloxane, reinforcing filler and molecular structure control agent into a kneader and stir them evenly at room temperature; Step 2: After the stirring is completed, the materials in step 1 are placed in a kneader and refined under a vacuum environment to form a base rubber; Step 3: Divide the base glue into two parts, add a catalyst to one part, stir evenly at room temperature to form glue A; add hydrogen-containing silicone oil and a catalyst to the other part, stir evenly at room temperature to form glue B; Step 4: Mix glue A and glue B together, stir and vulcanize to form the finished product.

8. A process for preparing low-temperature fast-vulcanizing liquid silicone rubber according to claim 7, It is characterized in that In the step 1, the stirring time at room temperature is 1.5-2 hours.

9. A process for preparing low-temperature fast-vulcanizing liquid silicone rubber according to claim 8, It is characterized in that In the step 2, the temperature in the vacuum environment is 160° C.-180° C., and the refining time is 2 hours.

Citation Information

Patent Citations

  • Self-adhesive single-component addition-type silicone rubber and preparation method thereof

    CN110387128A

  • Preparation method of silica-containing alkoxy boron siloxane modified white carbon black and application thereof

    CN112094434A

  • Two-component addition type room temperature vulcanization mold silicone rubber and preparation method thereof

    CN115246990A

  • Low-temperature bonding boiling-resistant double-component addition type silicone rubber and preparation method thereof

    CN115521625A

  • Macromolecular alkoxy silane treating agent with T-shaped symmetrical structure as well as preparation method and application of macromolecular alkoxy silane treating agent

    CN116082641A