Anti-static fireproof inorganic silicate coating as well as preparation method and application thereof
Through the combination of modified potassium silicate and antistatic agent, the problem of insufficient antistatic and fire-proof performance of inorganic coatings in the northwest region is solved, and efficient and economical coating preparation is achieved. It is suitable for building facilities in the northwest region and has good fire protection and anti-static properties.
Patent Information
- Application Number
- CN202411386374.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The existing inorganic coatings have problems with insufficient anti-static and fire-proof performance in the applications of the Northwest region, and the addition of additives in traditional methods leads to increased costs and poor weather resistance, which makes it difficult to meet regional needs.
By using a combination of modified potassium silicate and antistatic agent, an anti-static inorganic silicate coating suitable for the northwest region is prepared, and the fire resistance of the coating is improved by using organic fluorine shells, and through conductive sericite and polyaniline The layer enhances conductivity, combines hydrophobic cellulose and functional additives to achieve good compatibility and stability of the coating.
It significantly improves the anti-static and fire-proof performance of inorganic silicate coatings, achieves A-level combustion performance, has the advantages of energy saving, environmental protection, anti-corrosion, mildew resistance, etc. It is suitable for densely populated public places and meets the coating needs of the Northwest region.
Smart Images

Figure BDA0005071064720000191 
Figure BDA0005071064720000201 
Figure BDA0005071064720000202
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an antistatic and fireproof inorganic silicate coating and a preparation method and application thereof. Background Art
[0002] Due to the large differences in atmospheric composition, cloud cover, and atmospheric water vapor between the eastern and western regions of my country, the coating effect of the same paint in different regions varies greatly. According to statistics, the annual average total ground solar radiation in the eastern region from 1961 to 2011 was 4910.83MJ / m 2 During the same period, the total solar radiation in the western region reached 6058.12 MJ / m 2 On the other hand, according to the National Bureau of Statistics, the average relative humidity in the capital cities of eastern my country reached 67.1% in 2022, while the average relative humidity in the five northwestern provinces was only 53%. In addition, there are obvious differences in sunshine duration, temperature difference, and atmospheric suspended matter. This difference makes it easy for the coating formulas in the eastern region to be obviously "unsuitable" in the northwest region.
[0003] Therefore, in order to achieve the desired coating effect, paint workers have to increase the type and amount of additives to achieve a relatively ideal coating effect, but this process often leads to problems such as poor weather resistance of coating products, increased volatile organic compound content and increased costs. Based on this situation, developing a coating with appropriate material ratio and low volatile organic compound content is of great significance to meet the production and life needs of people in the northwest region.
[0004] When water-based inorganic coatings are applied on surfaces such as cement mortar, concrete and masonry, they are firmly bonded to the wall through petrochemical reactions without obvious interfaces. Therefore, they have better air permeability, pollution resistance, antibacterial properties, fire retardancy and good comprehensive environmental protection performance. In recent years, water-based inorganic coatings have become the new favorite in the coatings market. With the development of society, people have higher and higher requirements for coating functions. Especially for building facilities in the western region (such as residential buildings or public buildings such as schools, hospitals, theaters, etc.), the application of anti-static functions may greatly improve safety and comfort. On the other hand, GB 50222-2017 "Fire Protection Code for Interior Decoration Design of Buildings" has clear requirements for the flammability of decorative materials for civil buildings, warehouses, factories and walls, and most of them require Class A non-combustibility. However, there are very few coating products on the market that are both anti-static and fireproof, and the effects of anti-static and / or fireproof products are poor.
[0005] The antistatic function of traditional inorganic coatings is mainly achieved by adding metal and carbon conductive fillers, but metal fillers are easily oxidized and have dark colors; carbon fillers have a single color and are difficult to process. Relatively speaking, light-colored metal oxide fillers have good conductivity through surface modification, and their raw materials are simple and easy to obtain, such as titanium dioxide, mica powder, etc., and have broad development and application prospects. On the other hand, traditional inorganic coatings require the addition of organic defoamers, wetting agents, thickeners and other additives due to their film stability requirements, resulting in poor fire retardancy. These problems have greatly limited the application of inorganic coatings in industry.
[0006] In view of the shortcomings of the above methods, it is of great significance to develop an anti-static and fire-proof inorganic silicate coating suitable for the northwest region and a preparation method thereof.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] The purpose of the present invention is to provide an antistatic and fireproof inorganic silicate coating and a preparation method and application thereof. The present invention obtains an antistatic and fireproof inorganic silicate coating suitable for the northwest region by adding modified potassium silicate with a specific structure and an antistatic agent, which significantly improves the antistatic and fireproof properties of the inorganic silicate coating while saving costs.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] In a first aspect, the present invention provides an antistatic and fireproof inorganic silicate coating, wherein the raw materials for preparing the antistatic and fireproof inorganic silicate coating include, by weight: 25 to 40 parts of modified potassium silicate, 35 to 70 parts of filler, 0.2 to 0.8 parts of cellulose, 0.1 to 0.5 parts of antistatic agent, 1 to 20 parts of functional additive, and 15 to 23 parts of water;
[0011] The modified potassium silicate comprises a potassium silicate core and an organic fluorine shell layer coated on the surface of the potassium silicate core;
[0012] The antistatic agent comprises conductive sericite and a polyaniline layer deposited on the surface of the conductive sericite.
[0013] Preferably, the raw materials for preparing the modified potassium silicate include, by weight:
[0014] 2 to 4 parts of acrylate monomers, 2 to 4 parts of fluorine-containing vinyl monomers, 15-30 parts of alkaline potassium silicate sol, 0.03 to 0.1 parts of organic silicon coupling agents, 0.1 to 1 parts of initiators, and 1 to 10 parts of solvents.
[0015] Preferably, the acrylic ester monomer is butyl acrylate.
[0016] Preferably, the fluorine-containing vinyl monomer is 1,1-difluoroethylene and / or trifluoroethylene.
[0017] Preferably, the alkaline potassium silicate sol has a pH of 9 to 10 and a solid content of 20 to 40 wt%.
[0018] Preferably, the organic silicon coupling agent is γ-methacryloxypropyltrimethoxysilane.
[0019] Preferably, the initiator is dibenzoyl peroxide.
[0020] Preferably, the solvent is ethylene glycol monobutyl ether.
[0021] Preferably, the modified potassium silicate is prepared by the following steps:
[0022] After dissolving the first part of the initiator in the solvent, heating to 80-120° C., a raw material solution 1 is obtained;
[0023] Mixing an acrylic acid ester monomer, a fluorine-containing vinyl monomer and a second part of an initiator to obtain a second raw material solution, and dripping the second raw material solution into the first raw material solution;
[0024] After the second raw material solution has been added for 10 to 20 minutes, the mixed solution of alkaline potassium silicate sol and organosilicon coupling agent is added to the first raw material solution simultaneously, and the adding time is controlled to be 1 to 3 hours;
[0025] After the dropwise addition is completed, the remaining initiator is added to the mixed solution, and a constant temperature reaction is carried out at 105 to 115° C. for 0.5 to 1.5 hours to obtain the modified potassium silicate.
[0026] Preferably, the mass ratio of the first part of initiator, the second part of initiator and the remaining initiator is 2:1:1.
[0027] Preferably, after the isothermal reaction is completed, the following steps are further included: reducing the temperature of the reaction solution after the isothermal reaction to below 45° C., adjusting the pH of the solution to 7-8, and obtaining the modified potassium silicate.
[0028] Preferably, the raw materials for preparing the antistatic agent include, by weight: 4 to 6 parts of conductive sericite, 0.4 to 0.6 parts of p-phenylenediamine, 0.1 to 0.12 parts of phosphoric acid, and 4 to 6 parts of initiator.
[0029] Preferably, the initiator is dibenzoyl peroxide.
[0030] Preferably, the conductive sericite comprises sericite and a conductive oxide layer deposited on the surface of the sericite.
[0031] Preferably, the raw materials for preparing the conductive sericite include, by weight:
[0032] 8-11 parts of tin salt, 1-3 parts of antimony salt, 18-23 parts of sericite, 30-35 parts of acid solution, 4-7 parts of sodium tripolyphosphate solution, and 30-40 parts of alkali solution.
[0033] Preferably, the tin salt is tin tetrachloride.
[0034] Preferably, the antimony salt is antimony trichloride.
[0035] Preferably, the acid solution is a 10-20 wt % hydrochloric acid aqueous solution.
[0036] Preferably, the sodium tripolyphosphate solution is a 20-40 wt % sodium tripolyphosphate aqueous solution.
[0037] Preferably, the alkali solution is a 10-20 wt % sodium hydroxide aqueous solution.
[0038] Preferably, the antistatic agent is prepared by the following steps:
[0039] Dispersing sericite in water to obtain a sericite suspension; mixing tin salt, antimony salt and acid solution to obtain a mixed solution; simultaneously dropping the mixed solution and alkali solution into the sericite suspension to react at 10-40° C. for 0.5-1.5 hours to obtain a first reaction solution; dropping sodium tripolyphosphate solution into the first reaction solution, stirring at 10-40° C. for 0.5-1.5 hours, filtering, washing and drying in sequence, and calcining at 750-850° C. for 4-6 hours to obtain the conductive sericite;
[0040] Dispersing conductive sericite in water to obtain a conductive sericite dispersion; adding p-phenylenediamine and phosphoric acid to the conductive sericite dispersion, stirring at 10 to 40° C. for 0.5 to 1.5 hours to obtain a mixed solution; dissolving an initiator in water to obtain an initiator solution; dropping the initiator solution into the mixed solution, stirring at 10 to 40° C. for 6 to 18 hours, and then filtering, washing, drying, crushing and grinding to obtain the antistatic agent.
[0041] Preferably, the filler includes any one of titanium dioxide, heavy calcium or sericite, or a combination of at least two of them.
[0042] Preferably, the filler comprises, by weight: 20 to 30 parts of titanium dioxide, 15 to 30 parts of heavy calcium, and 3 to 10 parts of sericite.
[0043] Preferably, the mesh size of the heavy calcium is 800-1250 meshes.
[0044] Preferably, the cellulose is a hydrophobic hydroxyalkyl modified cellulose, preferably a hydrophobic hydroxyethyl modified cellulose.
[0045] Preferably, the cellulose has a hydroxyl content of 18-23%, and an ethyl content of 5-7%.
[0046] Preferably, the cellulose includes any one of 250HRR, 250HHBR, HE10K, M-100, 30000H or HS10, or a combination of at least two thereof.
[0047] Preferably, the functional additive includes any one of a dispersant, a stabilizer, a defoamer, a toughening agent, an anti-settling agent, a deodorizing emulsion, a leveling agent or a water-resistant agent, or a combination of at least two thereof.
[0048] Preferably, the functional additives include, by weight: 0.2-0.6 parts of dispersant, 0.1-1 parts of stabilizer, 0.1-1 parts of defoamer, 0.1-1 parts of toughening agent, 0.1-1 parts of anti-settling agent, 1-8 parts of deodorizing emulsion, 0.1-1 parts of leveling agent and 0.1-1 parts of water-resistant agent.
[0049] Preferably, the dispersant includes any one of a sodium salt dispersant, an ammonium salt dispersant or a high molecular polymer dispersant, or a combination of at least two of them.
[0050] Preferably, the stabilizer is silica sol.
[0051] Preferably, the defoamer includes any one of a mineral oil defoamer, a silicone defoamer, a polyether defoamer or a polyether-modified silicone defoamer, or a combination of at least two of them.
[0052] Preferably, the toughening agent is vinyl acetate-ethylene copolymer emulsion.
[0053] Preferably, the anti-settling agent is water-based polyamide.
[0054] Preferably, the deodorizing emulsion includes any one of styrene acrylic emulsion, silicone acrylic emulsion, acrylate emulsion, polyvinyl acetate emulsion, ethylene vinyl acetate emulsion or ethylene acrylate emulsion, or a combination of at least two thereof.
[0055] Preferably, the leveling agent is a polyurethane leveling agent.
[0056] Preferably, the water-resistant agent is polyethylene wax emulsion.
[0057] In a second aspect, the present invention provides a method for preparing the antistatic and fireproof inorganic silicate coating as described in the first aspect, the preparation method comprising:
[0058] Modified potassium silicate, filler, cellulose, antistatic agent and functional additive are dispersed in water according to a proportion to obtain the antistatic and fireproof inorganic silicate coating.
[0059] Preferably, the preparation method specifically comprises the following steps:
[0060] (1) adding cellulose, a dispersant, a stabilizer and a defoamer into water for a first dispersion to obtain a mixed solution 1;
[0061] (2) adding a filler, an antistatic agent, a toughening agent and an anti-settling agent to the mixed solution 1, and performing a second dispersion to obtain a mixed solution 2;
[0062] (3) adding a deodorizing emulsion, a leveling agent and a portion of modified potassium silicate to the mixed solution 2, scraping and stirring to obtain a mixed solution 3;
[0063] (4) Adding a water-resistant agent and the remaining modified potassium silicate to the mixed solution 3, stirring the mixture, and obtaining the antistatic and fireproof inorganic silicate coating.
[0064] Preferably, in step (1), the rotation speed of the first dispersion is 300-500 r / min.
[0065] Preferably, in step (2), the rotation speed of the second dispersion is 1500-2500 r / min, and the time of the second dispersion is more than 20 min.
[0066] Preferably, in step (2), the fineness of the particles in the second mixed solution is less than 50 μm.
[0067] Preferably, in step (3), the mass of the modified potassium silicate accounts for 20-40% of the total mass of the modified potassium silicate.
[0068] Preferably, in step (3), the stirring speed is 300 to 500 r / min.
[0069] Preferably, in step (3), the pH of the mixed solution three is above 11.
[0070] Preferably, in step (4), the stirring speed is 500-800 r / min.
[0071] In a third aspect, the present invention provides an application of the antistatic and fireproof inorganic silicate coating as described in the first aspect in the protection of building facilities in the northwest region.
[0072] Compared with the prior art, the present invention has the following beneficial effects:
[0073] (1) The modified potassium silicate of the present invention uses organic fluorine to coat potassium silicate to form a core-shell structure, and uses strong carbon-fluorine bond energy to arrange fluorine atoms closely around the carbon main chain, thereby improving the strength and performance of the inorganic coating film, achieving the A1 level in the A level of combustion performance, and satisfying the combustion value PCS of the inorganic coating ≤2.0MJ / Kg, and the continuous combustion time = 0s.
[0074] (2) The antistatic agent of the present invention is selected to deposit or coat a conductive oxide layer on the surface of the conductive sericite, which has good suspension performance, is not easy to settle, and is easier to disperse.
[0075] (3) The cellulose described in the present invention uses hydrophobic hydroxyethyl modified cellulose to improve the storage stability of water-based inorganic coatings, and has excellent thixotropy, suspension and compatibility. Structurally, its hydrophobic main chain and surrounding water molecules are hydrogen-bonded with the organic phase and aqueous phase in the coating, respectively, and can be well compatible with the wetting agents and dispersants of various color paste systems, effectively preventing the sinking of pigments and fillers in water-based inorganic coatings and the floating color of color pastes.
[0076] (4) The filler of the present invention is preferably a combination of titanium dioxide, heavy calcium and sericite, and is supplemented with functional additives (such as stabilizers, toughening agents, anti-settling agents, and water-resistant agents). The good compatibility between the components enables a good coating effect to be achieved with a relatively small amount of reagents. The prepared coating is well adapted to the coating needs of residential buildings and public places in the northwest region.
[0077] (5) The inorganic coating of the present invention has the advantages of energy saving and economy, environmental protection and non-toxicity, flame retardant or non-flammable, anti-corrosion and mildew resistance, acid corrosion resistance, good air permeability, dustproof and self-cleaning, super durability and anti-static. It is a product that meets the requirements of environmental protection and high quality performance, and is very suitable for use in densely populated places such as airports, schools, hospitals, subway stations, theaters, etc. DETAILED DESCRIPTION
[0078] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0079] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0080] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] In a first aspect, the present invention provides an antistatic and fireproof inorganic silicate coating, wherein the raw materials for preparing the antistatic and fireproof inorganic silicate coating include, by weight: 25 to 40 parts of modified potassium silicate, 35 to 70 parts of filler, 0.2 to 0.8 parts of cellulose, 0.1 to 0.5 parts of antistatic agent, 1 to 20 parts of functional additive, and 15 to 23 parts of water;
[0082] The modified potassium silicate comprises a potassium silicate core and an organic fluorine shell layer coated on the surface of the potassium silicate core;
[0083] The antistatic agent comprises conductive sericite and a polyaniline layer deposited on the surface of the conductive sericite.
[0084] The present invention obtains an antistatic and fireproof inorganic silicate coating suitable for the northwest region by adding modified potassium silicate and antistatic agent of specific structure, so that the antistatic and fireproof performance of inorganic silicate coating is significantly improved while saving cost. Among them, the modified potassium silicate uses organic fluorine to coat potassium silicate to form a core-shell structure, and uses strong carbon-fluorine bond energy to make fluorine atoms closely arranged around the carbon main chain, thereby improving the strength and performance of the inorganic coating film, reaching the A1 level in the combustion performance A level, and meeting the combustion value PCS of inorganic coating ≤2.0MJ / Kg, and the continuous burning time = 0s. At the same time, the antistatic agent of the present invention is selected to deposit or coat a conductive oxide layer on the surface of conductive sericite to enhance the conductivity of the conductive sericite itself, and has good suspension performance, is not easy to settle, and is easier to disperse.
[0085] As an optional embodiment of the present invention, in the preparation raw materials of the inorganic silicate coating, the content of modified potassium silicate is 25 to 40 parts, for example, it can be 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, etc.
[0086] As an optional embodiment of the present invention, the content of filler in the preparation raw materials of the inorganic silicate coating is 35 to 70 parts, for example, it can be 35 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, 68 parts, 70 parts, etc.
[0087] As an optional embodiment of the present invention, the content of cellulose in the raw materials for preparing the inorganic silicate coating is 0.2 to 0.8 parts, for example, it can be 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, etc.
[0088] As an optional embodiment of the present invention, the content of the antistatic agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 0.5 parts, for example, it can be 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, etc.
[0089] As an optional embodiment of the present invention, the content of the functional additive in the preparation raw materials of the inorganic silicate coating is 1 to 20 parts, for example, it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0090] As an optional embodiment of the present invention, the water content in the raw materials for preparing the inorganic silicate coating is 15 to 23 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, etc.
[0091] As an optional embodiment of the present invention, the raw materials for preparing the modified potassium silicate include, by weight: 2 to 4 parts of acrylate monomers, 2 to 4 parts of fluorine-containing vinyl monomers, 15-30 parts of alkaline potassium silicate sol, 0.03 to 0.1 parts of organosilicon coupling agents, 0.1 to 1 parts of initiators, and 1 to 10 parts of solvents.
[0092] In the present invention, the modified potassium silicate is an organic fluorine resin modified potassium silicate emulsion prepared by copolymerization of the above-mentioned specific proportions of the raw materials, and uses acrylate monomers and fluorine-containing vinyl monomers to form chemical bonds between organic polymers and inorganic particles, thereby achieving the coating of potassium silicate with active organic fluorine resin to form a core-shell structure, and using strong carbon-fluorine bond energy to make fluorine atoms closely arranged around the carbon main chain, thereby improving the strength and fire resistance of the inorganic coating film.
[0093] As an optional embodiment of the present invention, in the preparation raw material of modified potassium silicate, the content of acrylate monomer is 2 to 4 parts, for example, it can be 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, etc.
[0094] As an optional embodiment of the present invention, the content of fluorine-containing vinyl monomer in the raw material for preparing modified potassium silicate is 2 to 4 parts, for example, it can be 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, etc.
[0095] As an optional embodiment of the present invention, in the raw material for preparing modified potassium silicate, the content of alkaline potassium silicate sol is 15-30 parts, for example, it can be 15 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, etc.
[0096] As an optional embodiment of the present invention, the content of the organosilicon coupling agent in the preparation raw material of the modified potassium silicate is 0.03 to 0.1 parts, for example, it can be 0.03 parts, 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 0.1 parts, etc.
[0097] As an optional embodiment of the present invention, the content of the initiator in the preparation raw material of modified potassium silicate is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0098] As an optional embodiment of the present invention, the content of the solvent in the raw material for preparing the modified potassium silicate is 1 to 10 parts, for example, it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0099] As an optional embodiment of the present invention, in the raw material for preparing the modified potassium silicate, the acrylic ester monomer is butyl acrylate.
[0100] As an optional embodiment of the present invention, in the raw material for preparing the modified potassium silicate, the fluorine-containing vinyl monomer is 1,1-difluoroethylene and / or trifluoroethylene.
[0101] As an optional embodiment of the present invention, in the raw material for preparing modified potassium silicate, the pH of the alkaline potassium silicate sol is 9-10, for example, it can be 9, 9.2, 9.4, 9.6, 9.8, 10, etc.
[0102] As an optional embodiment of the present invention, the solid content of the alkaline potassium silicate sol is 20-40wt%, for example, it can be 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt% and the like.
[0103] In the present invention, the alkaline potassium silicate sol is a colloidal solution of silicon dioxide particles in a potassium hydroxide aqueous solution. The colloidal particles have a diameter of nanometer level, a large surface area, low viscosity, and good dispersibility and permeability.
[0104] As an optional embodiment of the present invention, in the raw material for preparing the modified potassium silicate, the organic silicon coupling agent is γ-methacryloxypropyltrimethoxysilane (KH-570).
[0105] As an optional embodiment of the present invention, in the raw material for preparing the modified potassium silicate, the initiator is dibenzoyl peroxide (BPO).
[0106] As an optional embodiment of the present invention, in the raw material for preparing modified potassium silicate, the solvent is ethylene glycol monobutyl ether.
[0107] As an optional embodiment of the present invention, the modified potassium silicate is prepared by the following steps:
[0108] (a) dissolving the first part of the initiator in a solvent and heating the solvent to 80-120° C. to obtain a raw material solution 1;
[0109] (b) mixing an acrylic acid ester monomer, a fluorine-containing vinyl monomer and a second part of an initiator to obtain a second raw material solution, and dropwise adding the second raw material solution into the first raw material solution;
[0110] (c) After the second raw material solution has been added for 10 to 20 minutes, the mixed solution of alkaline potassium silicate sol and organosilicon coupling agent is added to the first raw material solution simultaneously, and the addition time is controlled to be 1 to 3 hours;
[0111] (d) After the dropwise addition is completed, the remaining initiator is added to the mixed solution, and a constant temperature reaction is carried out at 105-115° C. for 0.5-1.5 h to obtain the modified potassium silicate.
[0112] In the present invention, the modified potassium silicate is prepared by the above-mentioned method. When the acrylic ester monomers and the fluorine-containing vinyl monomers are copolymerized under the action of an initiator, the generated free radicals can be attracted to the surface of the nano-SiO2 particles, so that a chemical bond is formed between the organic polymer and the inorganic particles, and the active organic fluorine resin is coated on the potassium silicate to form a core-shell structure; at the same time, the carbon-fluorine bond energy is relatively strong, and the fluorine atoms are closely arranged around the carbon main chain, thereby improving the fire retardant performance of the inorganic coating.
[0113] As an optional embodiment of the present invention, in step (a), heating is performed to 80-120°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 115°C, 120°C, etc.
[0114] As an optional embodiment of the present invention, in step (c), after the second drop of the raw material solution is added for 10 to 20 minutes, for example, it can be 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes, 20 minutes, etc.
[0115] As an optional embodiment of the present invention, in step (c), the dropping time is controlled to be 1 to 3 hours, for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, etc.
[0116] It should be noted that after 10 to 20 minutes of dropwise addition of the raw material solution 2, some of the raw material solution 2 is not completely added. The raw material solution 2 is added to the raw material solution 1 through a device containing a mixed solution of alkaline potassium silicate sol and an organosilicon coupling agent. At the same time, the remaining raw material solution 2 is also added dropwise. The dropping speed is controlled so that the remaining raw material solution 2, the mixed solution of alkaline potassium silicate sol and the organosilicon coupling agent are added dropwise within 1 to 3 hours.
[0117] As an optional embodiment of the present invention, the mass ratio of the first part of initiator, the second part of initiator and the remaining initiator is 2:1:1.
[0118] As an optional embodiment of the present invention, after the isothermal reaction is completed, the following steps are further included:
[0119] The temperature of the reaction solution after the isothermal reaction is reduced to below 45°C (for example, it can be 45°C, 44°C, 43°C, 42°C, 41°C, 40°C, 38°C, 35°C, etc.), and the pH of the solution is adjusted to 7-8 (for example, it can be 7, 7.2, 7.4, 7.6, 7.8, 8, etc.) to obtain the modified potassium silicate.
[0120] As an optional embodiment of the present invention, the raw materials for preparing the antistatic agent include, by weight: 4-6 parts of conductive sericite, 0.4-0.6 parts of p-phenylenediamine, 0.1-0.12 parts of phosphoric acid, 4-6 parts of initiator and 0.6-0.8 parts of water.
[0121] As an optional embodiment of the present invention, the content of conductive sericite in the raw materials for preparing the antistatic agent is 4 to 6 parts, for example, it can be 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts, 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, etc.
[0122] As an optional embodiment of the present invention, the content of p-phenylenediamine in the raw materials for preparing the antistatic agent is 0.4 to 0.6 parts, for example, it can be 0.4 parts, 0.42 parts, 0.44 parts, 0.46 parts, 0.48 parts, 0.5 parts, 0.52 parts, 0.54 parts, 0.56 parts, 0.58 parts, 0.6 parts, etc.
[0123] As an optional embodiment of the present invention, the content of phosphoric acid in the raw material for preparing the antistatic agent is 0.1 to 0.12 parts, for example, it can be 0.1 parts, 0.105 parts, 0.11 parts, 0.115 parts, 0.12 parts, etc.
[0124] As an optional embodiment of the present invention, the content of the initiator in the raw materials for preparing the antistatic agent is 4 to 6 parts, for example, it can be 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts, 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, etc.
[0125] As an optional embodiment of the present invention, the water content in the raw material for preparing the antistatic agent is 0.6-0.8 parts, for example, it can be 0.6 parts, 0.62 parts, 0.64 parts, 0.66 parts, 0.68 parts, 0.7 parts, 0.72 parts, 0.74 parts, 0.78 parts, 0.8 parts, etc.
[0126] As an optional embodiment of the present invention, in the raw materials for preparing the antistatic agent, the initiator is dibenzoyl peroxide.
[0127] As an optional embodiment of the present invention, the conductive sericite includes sericite and a conductive oxide layer deposited on the surface of the sericite.
[0128] As an optional embodiment of the present invention, the raw materials for preparing the conductive sericite include, by weight: 8-11 parts of tin salt, 1-3 parts of antimony salt, 18-23 parts of sericite, 30-35 parts of acid solution, 4-7 parts of sodium tripolyphosphate solution, and 30-40 parts of alkali solution.
[0129] As an optional embodiment of the present invention, the content of tin salt in the raw material for preparing conductive sericite is 8 to 11 parts, for example, it can be 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 10.5 parts, 11 parts, etc.
[0130] As an optional embodiment of the present invention, the content of antimony salt in the raw material for preparing conductive sericite is 1 to 3 parts, for example, it can be 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.3 parts, 2.5 parts, 2.7 parts, 3 parts, etc.
[0131] As an optional embodiment of the present invention, the content of sericite in the raw material for preparing conductive sericite is 18 to 23 parts, for example, it can be 18 parts, 18.5 parts, 19 parts, 19.5 parts, 20 parts, 20.5 parts, 21 parts, 21.5 parts, 22 parts, 22.5 parts, 23 parts, etc.
[0132] As an optional embodiment of the present invention, the content of acid solution in the preparation raw material of conductive sericite is 30-35 parts, for example, it can be 30 parts, 30.5 parts, 31 parts, 31.5 parts, 32 parts, 32.5 parts, 33 parts, 33.5 parts, 34 parts, 34.5 parts, 35 parts, etc.
[0133] As an optional embodiment of the present invention, the raw material for preparing the conductive sericite includes 4 to 7 parts of sodium tripolyphosphate solution, for example, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, etc.
[0134] As an optional embodiment of the present invention, the content of alkali solution in the preparation raw material of conductive sericite is 30-40 parts, for example, it can be 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, etc.
[0135] As an optional embodiment of the present invention, in the raw material for preparing conductive sericite, the tin salt is tin tetrachloride.
[0136] As an optional embodiment of the present invention, in the raw material for preparing conductive sericite, the antimony salt is antimony trichloride.
[0137] As an optional embodiment of the present invention, the acid solution is a 10-20wt% hydrochloric acid aqueous solution, for example, it can be 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt% and the like.
[0138] As an optional embodiment of the present invention, the sodium tripolyphosphate solution is a 20-40wt% sodium tripolyphosphate aqueous solution, for example, it can be 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt% and the like.
[0139] As an optional embodiment of the present invention, the alkali solution is a 10-20wt% sodium hydroxide aqueous solution, for example, it can be 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt% and the like.
[0140] As an optional embodiment of the present invention, the antistatic agent is prepared by the following steps:
[0141] (A) dispersing sericite in water to obtain a sericite suspension; mixing a tin salt, an antimony salt and an acid solution to obtain a mixed solution; simultaneously dropping the mixed solution and an alkali solution into the sericite suspension to react at 10 to 40° C. for 0.5 to 1.5 hours to obtain a reaction solution 1; dropping a sodium tripolyphosphate solution into the reaction solution 1, stirring at 10 to 40° C. for 0.5 to 1.5 hours, filtering, washing, drying in sequence, and calcining at 750 to 850° C. for 4 to 6 hours to obtain the conductive sericite;
[0142] (B) dispersing conductive sericite in water to obtain a conductive sericite dispersion; adding p-phenylenediamine and phosphoric acid to the conductive sericite dispersion, stirring at 10 to 40° C. for 0.5 to 1.5 hours to obtain a mixed solution; dissolving an initiator in water to obtain an initiator solution; dropping the initiator solution into the mixed solution, stirring at 10 to 40° C. for 6 to 18 hours, and then filtering, washing, drying, crushing and grinding to obtain the antistatic agent.
[0143] In the preparation process of the antistatic agent of the present invention, a conductive oxide layer is first formed on the surface of sericite by nanotechnology in step (A) to obtain the conductive sericite, and then p-phenylenediamine is polymerized on the surface to form a stable conductive layer in step (B) to obtain the antistatic agent. The antistatic agent of the present invention introduces a polyaniline structure having both "benzene-benzene" and "benzene-quinone" structures on the surface of the conductive sericite through the polymerization process, further enhancing the conductivity of the conductive sericite itself, and polyaniline can protect the metal through its coordination with the metal, and has good chemical stability.
[0144] As an optional embodiment of the present invention, in step (A), after the sodium tripolyphosphate solution is added dropwise to the reaction solution 1, the stirring temperature is 10-40°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0145] As an optional embodiment of the present invention, in step (A), after the sodium tripolyphosphate solution is added dropwise to the reaction solution 1, the stirring time is 0.5 to 1.5 h, for example, 0.5 h, 0.6 h, 0.8 h, 1.0 h, 1.2 h, 1.4 h, 1.5 h, etc.
[0146] As an optional embodiment of the present invention, in step (A), after the sodium tripolyphosphate solution is added dropwise to the reaction solution 1, the stirring temperature is 10-40°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0147] As an optional embodiment of the present invention, in step (A), after the sodium tripolyphosphate solution is added dropwise to the reaction solution 1, the stirring time is 0.5 to 1.5 h, for example, 0.5 h, 0.6 h, 0.8 h, 1.0 h, 1.2 h, 1.4 h, 1.5 h, etc.
[0148] As an optional embodiment of the present invention, in step (A), the calcination temperature is 750-850°C, for example, it can be 750°C, 760°C, 780°C, 800°C, 820°C, 840°C, 850°C, etc.
[0149] As an optional embodiment of the present invention, in step (A), the calcination time is 4 to 6 hours, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8h, 6h, etc.
[0150] As an optional embodiment of the present invention, in step (B), p-phenylenediamine and phosphoric acid are added to the conductive sericite dispersion, and the stirring temperature is 10-40°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0151] As an optional embodiment of the present invention, in step (B), p-phenylenediamine and phosphoric acid are added to the conductive sericite dispersion, and the stirring time is 0.5 to 1.5 hours, for example, 0.5 hours, 0.6 hours, 0.8 hours, 1.0 hours, 1.2 hours, 1.4 hours, 1.5 hours, etc.
[0152] As an optional embodiment of the present invention, in step (B), an initiator liquid is added dropwise to the mixed liquid, and the stirring temperature is 10-40°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0153] As an optional embodiment of the present invention, in step (B), an initiator liquid is added dropwise to the mixed liquid, and the stirring time is 6 to 18 hours, for example, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, etc.
[0154] As an optional embodiment of the present invention, the filler includes any one of titanium dioxide, heavy calcium or sericite, or a combination of at least two of them.
[0155] As an optional embodiment of the present invention, the filler comprises, by weight: 20 to 30 parts of titanium dioxide, 15 to 30 parts of heavy calcium, and 3 to 10 parts of sericite.
[0156] As an optional embodiment of the present invention, the content of titanium dioxide in the preparation raw materials of the inorganic silicate coating is 20 to 30 parts, for example, it can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.
[0157] As an optional embodiment of the present invention, the content of heavy calcium in the preparation raw materials of the inorganic silicate coating is 15 to 30 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.
[0158] As an optional embodiment of the present invention, the content of sericite in the raw materials for preparing the inorganic silicate coating is 3 to 10 parts, for example, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0159] As an optional embodiment of the present invention, the mesh size of the heavy calcium is 800-1250 meshes, for example, it can be 800 mesh, 850 mesh, 900 mesh, 1000 mesh, 1100 mesh, 1200 mesh, 1250 mesh, etc.
[0160] As an optional embodiment of the present invention, the cellulose is a hydrophobic hydroxyalkyl modified cellulose, preferably a hydrophobic hydroxyethyl modified cellulose.
[0161] In the present invention, the cellulose is a hydrophobic hydroxyalkyl modified cellulose, which improves the storage stability of the water-based inorganic coating, and has excellent thixotropy, suspension and compatibility. Structurally, the cellulose is hydrogen-bonded with the surrounding water molecules through its hydrophobic main chain and the organic phase and the aqueous phase in the coating respectively, and can be well compatible with the wetting agent and dispersant of each color paste system, effectively preventing the sinking of the pigments and fillers in the water-based inorganic coating and the floating color of the color paste.
[0162] As an optional embodiment of the present invention, the cellulose has a hydroxyl content of 18-23%, for example, 18%, 19%, 20%, 21%, 22%, 23%, etc.; the ethyl content is 5-7%, for example, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, 6.2%, 6.4%, 6.6%, 6.8%, 7%, etc.
[0163] As an optional embodiment of the present invention, the cellulose includes any one of 250HRR, 250HHBR, HE10K, M-100, 30000H or HS10, or a combination of at least two thereof.
[0164] As an optional embodiment of the present invention, the functional additive includes any one of a dispersant, a stabilizer, a defoamer, a toughening agent, an anti-settling agent, a deodorizing emulsion, a leveling agent or a water-resistant agent, or a combination of at least two thereof.
[0165] As an optional embodiment of the present invention, the functional additives include, by weight: 0.2 to 0.6 parts of dispersant, 0.1 to 1 parts of stabilizer, 0.1 to 1 parts of defoamer, 0.1 to 1 parts of toughening agent, 0.1 to 1 parts of anti-settling agent, 1 to 8 parts of deodorizing emulsion, 0.1 to 1 parts of leveling agent and 0.1 to 1 parts of water resistance agent.
[0166] As an optional embodiment of the present invention, the content of the dispersant in the raw materials for preparing the inorganic silicate coating is 0.2 to 0.6 parts, for example, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, etc.
[0167] As an optional embodiment of the present invention, the content of the stabilizer in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0168] As an optional embodiment of the present invention, the content of the defoaming agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0169] As an optional embodiment of the present invention, the content of the toughening agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0170] As an optional embodiment of the present invention, the content of the anti-settling agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0171] As an optional embodiment of the present invention, the content of the odor-free emulsion in the raw materials for preparing the inorganic silicate coating is 1 to 8 parts, for example, it can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, etc.
[0172] As an optional embodiment of the present invention, the content of the leveling agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0173] As an optional embodiment of the present invention, the content of the water-resistant agent in the preparation raw materials of the inorganic silicate coating is 0.1 to 1 part, for example, it can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, etc.
[0174] As an optional embodiment of the present invention, the dispersant includes any one of a sodium salt dispersant, an ammonium salt dispersant or a high molecular polymer dispersant, or a combination of at least two of them.
[0175] As an optional embodiment of the present invention, the dispersant includes but is not limited to sodium salt dispersant 5040, ammonium salt dispersant 5027 or polymer dispersant SN4500 and the like.
[0176] As an optional embodiment of the present invention, the stabilizer is silica sol.
[0177] As an optional embodiment of the present invention, the stabilizer includes but is not limited to silica sol 260 and / or silica sol 360, etc.
[0178] As an optional embodiment of the present invention, the defoamer includes any one of a mineral oil defoamer, a silicone defoamer, a polyether defoamer or a polyether-modified silicone defoamer, or a combination of at least two of them.
[0179] As an optional embodiment of the present invention, the defoaming agent includes but is not limited to NXZ, F11, F12, 9625, 9648, DF806 or A10.
[0180] As an optional embodiment of the present invention, the toughening agent is vinyl acetate-ethylene copolymer emulsion.
[0181] As an optional embodiment of the present invention, the toughening agent includes but is not limited to VAE emulsion 837 or 837-2.
[0182] As an optional embodiment of the present invention, the anti-settling agent is water-based polyamide.
[0183] As an optional embodiment of the present invention, the anti-settling agent includes but is not limited to water-based polyamide W320 or F316.
[0184] As an optional embodiment of the present invention, the deodorizing emulsion includes any one of styrene acrylic emulsion, silicone acrylic emulsion, acrylate emulsion, polyvinyl acetate emulsion, ethylene vinyl acetate emulsion or ethylene acrylate emulsion, or a combination of at least two thereof.
[0185] As an optional embodiment of the present invention, the odor-free emulsion includes but is not limited to Badful 7367, 7701 or Sunrise 6152 and the like.
[0186] As an optional embodiment of the present invention, the leveling agent is a polyurethane leveling agent.
[0187] As an optional embodiment of the present invention, the leveling agent includes but is not limited to hydrophilic modified polyurethane emulsion WH307.
[0188] As an optional embodiment of the present invention, the water-resistant agent is a polyethylene wax emulsion.
[0189] As an optional embodiment of the present invention, the water-resistant agent includes but is not limited to polyethylene wax emulsion F3500.
[0190] In a second aspect, the present invention provides a method for preparing the antistatic and fireproof inorganic silicate coating as described in the first aspect, the preparation method comprising:
[0191] Modified potassium silicate, filler, cellulose, antistatic agent and functional additive are dispersed in water according to a proportion to obtain the antistatic and fireproof inorganic silicate coating.
[0192] As an optional embodiment of the present invention, the preparation method of the antistatic and fireproof inorganic silicate coating specifically comprises the following steps:
[0193] (1) adding cellulose, a dispersant, a stabilizer and a defoamer into water for a first dispersion to obtain a mixed solution 1;
[0194] (2) adding a filler, an antistatic agent, a toughening agent and an anti-settling agent to the mixed solution 1, and performing a second dispersion to obtain a mixed solution 2;
[0195] (3) adding a deodorizing emulsion, a leveling agent and a portion of modified potassium silicate to the mixed solution 2, scraping and stirring to obtain a mixed solution 3;
[0196] (4) Adding a water-resistant agent and the remaining modified potassium silicate to the mixed solution 3, stirring the mixture, and obtaining the antistatic and fireproof inorganic silicate coating.
[0197] As an optional embodiment of the present invention, in step (1), the rotation speed of the first dispersion is 300-500 r / min, for example, it can be 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min, etc.
[0198] As an optional embodiment of the present invention, in step (2), the rotation speed of the second dispersion is 1500-2500 r / min, for example, it can be 1500 r / min, 1600 r / min, 1800 r / min, 2000 r / min, 2200 r / min, 2400 r / min, 2500 r / min, etc., and the time of the second dispersion is more than 20 min, for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.
[0199] As an optional embodiment of the present invention, in step (2), the fineness of the particles in the second mixed solution is less than 50 μm, for example, it can be 50 μm, 45 μm, 40 μm, 35 μm, 30 μm, 25 μm, 20 μm, 15 μm, 10 μm, etc.
[0200] As an optional embodiment of the present invention, in step (3), the mass of the modified potassium silicate accounts for 20% to 40% of the total mass of the modified potassium silicate, for example, it can be 20%, 25%, 30%, 35%, 40%, etc.
[0201] As an optional embodiment of the present invention, in step (3), the stirring speed is 300-500 r / min, for example, it can be 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min, etc.
[0202] As an optional embodiment of the present invention, in step (3), the pH of the mixed solution three is above 11, for example, it can be 11, 11.2, 11.4, 11.5, 11.8, 12, etc.
[0203] As an optional embodiment of the present invention, in step (4), the stirring speed is 500-800 r / min, for example, it can be 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min, 800 r / min, etc.
[0204] In a third aspect, the present invention provides an application of the antistatic and fireproof inorganic silicate coating as described in the first aspect in the protection of building facilities in the northwest region.
[0205] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0206] Preparation Example 1
[0207] This preparation example provides a modified potassium silicate, which is prepared by the following steps:
[0208] (a) 0.2 kg of initiator dibenzoyl peroxide (BPO) was dissolved in 5 L of ethylene glycol monobutyl ether, mixed and added to a three-necked flask with a stirring device and a condenser, and heated to 100° C. in a thermostatic device;
[0209] (b) weighing 6.5 kg of monomers (the mass ratio of butyl acrylate to 1,1-difluoroethylene is 1:1) and 0.1 kg of initiator dibenzoyl peroxide (BPO), stirring and mixing, and slowly adding dropwise to the three-necked flask of step (a) through a constant pressure separatory funnel;
[0210] (c) After about 15 minutes of dropwise addition, 21.6 kg of alkaline potassium silicate sol (pH 9.5, solid content 30 wt%) and 0.52 kg of organosilicon coupling agent (KH-570) were mixed and added dropwise to the three-necked flask through another constant pressure separatory funnel. The dropping speed was controlled so that the liquids in the two constant pressure separatory funnels were added dropwise within 2 hours;
[0211] (d) After the dropwise addition is completed, 0.1 kg of initiator dibenzoyl peroxide (BPO) is added again, and the temperature is controlled to be constant at about 110° C. for reaction for 1 hour. After the reaction is completed, the temperature is lowered to 40° C. and the pH is adjusted to 7.5 to obtain the modified potassium silicate.
[0212] Preparation Example 2
[0213] This preparation example provides a modified potassium silicate, which is prepared by the following steps:
[0214] (a) 2 kg of initiator dibenzoyl peroxide (BPO) was dissolved in 50 L of ethylene glycol monobutyl ether, mixed and added into a three-necked flask with a stirring device and a condenser, and heated to 100° C. in a thermostat;
[0215] (b) weighing 65 kg of monomers (the mass ratio of butyl acrylate to trifluoroethylene is 1:1) and 1 kg of initiator dibenzoyl peroxide (BPO), stirring and mixing, and then slowly adding them dropwise into a three-necked flask through a constant pressure separatory funnel;
[0216] (c) After about 15 minutes of dropwise addition, 270 kg of alkaline potassium silicate sol (pH 9.5, solid content 30 wt%) and 0.5 kg of organosilicon coupling agent (KH-570) were mixed and added dropwise to the three-necked flask through another constant pressure separatory funnel. The dropwise addition speed was controlled so that the liquids in the two constant pressure separatory funnels were added dropwise within 2 hours;
[0217] (d) After the dropwise addition is completed, 1 kg of initiator dibenzoyl peroxide (BPO) is added again, and the temperature is controlled to be constant at about 110° C. for reaction for 1 hour. After the reaction is completed, the temperature is lowered to about 40° C., and the pH is adjusted to 7.5 to obtain the modified potassium silicate.
[0218] Preparation Example 3
[0219] This preparation example provides a modified potassium silicate, which is prepared by the following steps:
[0220] (a) 0.2 kg of initiator dibenzoyl peroxide (BPO) was dissolved in 5 L of ethylene glycol monobutyl ether, mixed and added to a three-necked flask with a stirring device and a condenser, and heated to 90° C. in a thermostat;
[0221] (b) weighing 4 kg of monomer (the mass ratio of butyl acrylate to 1,1-difluoroethylene is 1:1) and 0.1 kg of initiator dibenzoyl peroxide (BPO), stirring and mixing, and slowly adding dropwise to the three-necked flask of step (a) through a constant pressure separatory funnel;
[0222] (c) After about 10 minutes of dropwise addition, 15 kg of alkaline potassium silicate sol (pH 9.5, solid content 30 wt%) and 0.03 kg of organosilicon coupling agent (KH-570) were mixed and added dropwise to the three-necked flask through another constant pressure separatory funnel. The dropwise addition speed was controlled so that the liquids in the two constant pressure separatory funnels were added dropwise within 2 hours;
[0223] (d) After the dropwise addition is completed, 0.1 kg of initiator dibenzoyl peroxide (BPO) is added again, and the temperature is controlled at about 100° C. to react for 1.5 hours. After the reaction is completed, the temperature is lowered to 40° C. and the pH is adjusted to 7 to obtain the modified potassium silicate.
[0224] Preparation Example 4
[0225] This preparation example provides a modified potassium silicate, which is prepared by the following steps:
[0226] (a) 0.2 kg of initiator dibenzoyl peroxide (BPO) was dissolved in 5 L of ethylene glycol monobutyl ether, mixed and added to a three-necked flask with a stirring device and a condenser, and heated to 90° C. in a thermostat;
[0227] (b) weighing 8 kg of monomer (the mass ratio of butyl acrylate to 1,1-difluoroethylene is 1:1) and 0.1 kg of initiator dibenzoyl peroxide (BPO), stirring and mixing, and slowly adding dropwise to the three-necked flask of step (a) through a constant pressure separatory funnel;
[0228] (c) After about 20 minutes of dropwise addition, 30 kg of alkaline potassium silicate sol (pH 9.5, solid content 30 wt%) and 0.1 kg of organosilicon coupling agent (KH-570) were mixed and added dropwise to the three-necked flask through another constant pressure separatory funnel. The dropwise addition speed was controlled so that the liquids in the two constant pressure separatory funnels were added dropwise within 2 hours;
[0229] (d) After the dropwise addition is completed, 0.1 kg of initiator dibenzoyl peroxide (BPO) is added again, and the temperature is controlled at about 100° C. to react for 1.5 hours. After the reaction is completed, the temperature is lowered to 40° C. and the pH is adjusted to 8 to obtain the modified potassium silicate.
[0230] Preparation Example 5
[0231] This preparation example provides a modified potassium silicate, which differs from Preparation Example 1 in that in step (b), butyl acrylate is replaced by an equal mass of methyl acrylate, and 1,1-difluoroethylene is replaced by an equal mass of vinyl fluoride, and the other steps are consistent with Preparation Example 1.
[0232] Preparation Example 6
[0233] This preparation example provides a modified potassium silicate, which differs from Preparation Example 1 in that in step (b), butyl acrylate monomer is not added, the content of 1,1-difluoroethylene is increased to 6.5 kg, and the other steps are consistent with Preparation Example 1.
[0234] Preparation Example 7
[0235] This preparation example provides an antistatic agent, which is prepared by the following steps:
[0236] (A) Sericite and pure water were mixed in a mass ratio of 1:1 to prepare a pre-activated sericite suspension (50 wt%); SnCl4·5H2O and SbCl3 were mixed in a mass ratio of 9:1, and 1 kg of the mixture was added to 3 kg of hydrochloric acid solution (11 wt%) to prepare a mixed solution; then, the above mixed solution was added to 4 kg of pre-activated sericite suspension (50 wt%); NaOH solution (10 wt%) was then added dropwise until the acidity and alkalinity remained constant (pH 10); after the reaction was completed at 20°C for 1 hour, 0.5 kg of Na5P3O 10 The solution (40 wt%) was stirred at 20°C for 1 h; filtered, washed, dried, and calcined at 800°C for 5 h to obtain conductive sericite;
[0237] (B) Weigh 0.5 kg of the above-mentioned conductive sericite mica and add it into 40 mL of distilled water to disperse for 0.5 h, then add 0.05 kg of p-phenylenediamine and 0.11 kg of phosphoric acid under stirring with a stirrer, stir for 1 h at room temperature, weigh 0.5 kg of initiator dibenzoyl peroxide (BPO) and dissolve it in 30 mL of water, and add it dropwise to the mixed solution, continue stirring at room temperature for 12 h, and terminate the reaction; after cooling to room temperature, filter with suction, wash, dry overnight, crush and grind to obtain the antistatic agent.
[0238] Preparation Example 8
[0239] This preparation example provides an antistatic agent, which is prepared by the following steps:
[0240] (A) Sericite and pure water were mixed in a mass ratio of 1:1 to prepare a pre-activated sericite suspension (50 wt%); SnCl4·5H2O and SbCl3 were mixed in a mass ratio of 8:2, and 1 kg of the mixture was added to 3 kg of hydrochloric acid solution (15 wt%) to prepare a mixed solution; then, the above mixed solution was added to 4.4 kg of pre-activated sericite suspension (50 wt%); NaOH solution (14 wt%) was then added dropwise until the acidity and alkalinity remained constant (pH 10); after the reaction was completed at 10°C for 1.5 h, 0.6 kg of Na5P3O 10 The solution (30 wt%) was stirred at 20°C for 1 h; filtered, washed, dried, and calcined at 780°C for 6 h to obtain conductive sericite;
[0241] (B) 0.4 kg of the above-mentioned conductive sericite was weighed and added into 40 mL of distilled water and dispersed for 0.5 h. Subsequently, 0.06 kg of p-phenylenediamine and 0.12 kg of phosphoric acid were added under stirring with a stirrer, and stirred for 1.5 h at room temperature. 0.4 kg of initiator dibenzoyl peroxide (BPO) was weighed and dissolved in 30 mL of water, and added dropwise into the mixture, and stirring was continued at room temperature for 10 h to terminate the reaction; after cooling to room temperature, the mixture was filtered, washed, dried overnight, crushed and ground to obtain the antistatic agent.
[0242] Preparation Example 9
[0243] This preparation example provides an antistatic agent, which is prepared by the following steps:
[0244] (A) Sericite and pure water were mixed in a mass ratio of 1:1 to prepare a pre-activated sericite suspension (50 wt%); SnCl4·5H2O and SbCl3 were mixed in a mass ratio of 10:1, and 1 kg of the mixture was added to 3 kg of hydrochloric acid solution (18 wt%) to prepare a mixed solution; then, the above mixed solution was added to 4.6 kg of pre-activated sericite suspension (50 wt%); NaOH solution (18 wt%) was then added dropwise until the acidity and alkalinity remained constant (pH 10); after the reaction was completed at 40°C for 0.5 h, 0.7 kg of Na5P3O 10 The solution (20 wt%) was stirred at 20°C for 1 h; filtered, washed, dried, and calcined at 820°C for 4 h to obtain conductive sericite;
[0245] (B) 0.6 kg of the above-mentioned conductive sericite was weighed and added into 40 mL of distilled water and dispersed for 0.5 h, then 0.04 kg of p-phenylenediamine and 0.1 kg of phosphoric acid were added under stirring with a stirrer, and stirred for 40 min at room temperature, 0.6 kg of initiator dibenzoyl peroxide (BPO) was weighed and dissolved in 30 mL of water, and added dropwise to the mixture, and stirring was continued at room temperature for 16 h to terminate the reaction; after cooling to room temperature, the mixture was filtered, washed, dried overnight, crushed and ground to obtain the antistatic agent.
[0246] Preparation Example 10
[0247] This preparation example provides an antistatic agent, which is different from Preparation Example 7 in that SnCl4·5H2O is not added in step (A), and the other steps are consistent with Preparation Example 7.
[0248] Preparation Example 11
[0249] This preparation example provides an antistatic agent, which differs from Preparation Example 7 in that SbCl3 is not added in step (A), and the other steps are consistent with Preparation Example 7.
[0250] Comparative Preparation Example 1
[0251] This preparation example provides a modified potassium silicate, which differs from Preparation Example 1 in that in step (b), 1,1-difluoroethylene is not added, the content of butyl acrylate monomer is increased to 6.5 kg, and the other steps are consistent with Preparation Example 1.
[0252] Comparative Preparation Example 2
[0253] This preparation example provides an antistatic agent, which is prepared by the following steps:
[0254] Sericite and pure water were mixed in a mass ratio of 1:1 to prepare a pre-activated sericite suspension (50 wt%); SnCl4·5H2O and SbCl3 were mixed in a mass ratio of 10:1, and 1 kg of the mixture was added to 3 kg of hydrochloric acid solution (18 wt%) to prepare a mixed solution; then, the above mixed solution was added to 4.6 kg of pre-activated sericite suspension (50 wt%); NaOH solution (18 wt%) was added dropwise until the acidity and alkalinity remained constant (pH 10); after the reaction was completed at 40°C for 0.5 h, 0.7 kg of Na5P3O 10 The solution (20 wt%) was stirred at 20°C for 1 h; filtered, washed, dried, and calcined at 820°C for 4 h to obtain conductive sericite;
[0255] Comparative Preparation Example 3
[0256] This preparation example provides an antistatic agent, which is prepared by the following steps:
[0257] 0.6 kg of ordinary sericite was weighed and added to 40 mL of distilled water for dispersion for 0.5 h, and then 0.04 kg of p-phenylenediamine and 0.1 kg of phosphoric acid were added under stirring with a stirrer, and stirred at room temperature for 40 min. 0.6 kg of initiator dibenzoyl peroxide (BPO) was weighed and dissolved in 30 mL of water, and added dropwise to the mixed solution, and stirring was continued at room temperature for 16 h to terminate the reaction; after cooling to room temperature, the mixture was filtered, washed, dried overnight, and crushed and ground to obtain the antistatic agent.
[0258] Example 1
[0259] This embodiment provides an antistatic and fireproof inorganic silicate coating, which comprises the following components by weight:
[0260]
[0261] Among them, the dispersant is sodium salt dispersant 5040, the stabilizer is silica sol 260, the defoaming agent is NXZ, the toughening agent is VAE emulsion 837, the anti-settling agent is water-based polyamide W320, the odor-free emulsion is Badfu 7367, the leveling agent is hydrophilic modified polyurethane emulsion WH307, and the water-resistant agent is polyethylene wax emulsion F3500.
[0262] The preparation method of the inorganic silicate coating described in this embodiment comprises the following steps:
[0263] (1) At room temperature, add 0.5 kg of cellulose, 0.4 kg of dispersant, 0.2 kg of stabilizer and 0.35 kg of defoamer into 18.5 kg of water and disperse evenly at a speed of 400 r / min;
[0264] (2) Add 0.2 kg antistatic agent, 15 kg titanium dioxide, 20 kg heavy calcium, 2.5 kg toughening powder, 5 kg sericite and 0.3 kg anti-settling agent to the above mixture, and mix them evenly at a high speed of 2000 r / min in a high-speed dispersing device to ensure that the fineness is less than 50 μm;
[0265] (3) At a speed of 400 r / min, add 2 kg of odor-free emulsion, 0.2 kg of polyurethane leveling agent and 12 kg of modified potassium silicate to the above mixture, and mix them evenly by scraping and stirring (the stirring speed is 400 r / min). After the pH value of the system is measured to be above 11, proceed to the next step;
[0266] (4) 24 kg of modified potassium silicate solution and 0.2 kg of water-resistant agent were added, and the mixture was slowly stirred and dispersed for a certain period of time (stirring speed was 600 r / min, and time was 70 min) to obtain a finished inorganic silicate coating.
[0267] The coating performance test described in this embodiment is shown in Table 1 below:
[0268] Table 1
[0269]
[0270] Example 2
[0271] This embodiment provides an antistatic and fireproof inorganic silicate coating, which comprises the following components by weight:
[0272]
[0273]
[0274] Among them, the dispersant is sodium salt dispersant 5040, the stabilizer is silica sol 260, the defoaming agent is NXZ, the toughening agent is VAE emulsion 837, the anti-settling agent is water-based polyamide W320, the odor-free emulsion is Badfu 7367, the leveling agent is hydrophilic modified polyurethane emulsion WH307, and the water-resistant agent is polyethylene wax emulsion F3500.
[0275] The preparation method of the inorganic silicate coating described in this embodiment comprises the following steps:
[0276] (1) At room temperature, 1 kg of cellulose, 0.8 kg of dispersant, 0.4 kg of stabilizer and 0.7 kg of defoamer were added to 40 kg of water and dispersed evenly at a speed of 400 r / min;
[0277] (2) Add 0.3 kg antistatic agent, 30 kg titanium dioxide, 40 kg heavy calcium, 5 kg toughening powder, 10 kg sericite and 0.6 kg anti-settling agent to the above mixture, and mix them evenly in a high-speed dispersing device at a speed of 2000 r / min for 30 minutes to ensure that the fineness is less than 50 μm;
[0278] (3) At a speed of 400 r / min, add 4 kg of odor-free emulsion, 0.4 kg of polyurethane leveling agent and 24 kg of modified potassium silicate to the above mixture, and mix them evenly by scraping and stirring (the stirring speed is 450 r / min). After the pH value of the system is measured to be above 11, proceed to the next step;
[0279] (4) Add 48 kg of modified potassium silicate solution and 0.4 kg of water-resistant agent, slowly stir and disperse for a certain period of time (stirring speed is 660 r / min, time is 55 min), and obtain the finished inorganic silicate coating.
[0280] The coating performance test described in this embodiment is shown in Table 2 below:
[0281] Table 2
[0282]
[0283] Example 3
[0284] This embodiment provides an antistatic and fireproof inorganic silicate coating, which comprises the following components by weight:
[0285]
[0286]
[0287] Among them, the dispersant is sodium salt dispersant 5040, the stabilizer is silica sol 260, the defoaming agent is NXZ, the toughening agent is VAE emulsion 837, the anti-settling agent is water-based polyamide W320, the odor-free emulsion is Badfu 7367, the leveling agent is hydrophilic modified polyurethane emulsion WH307, and the water-resistant agent is polyethylene wax emulsion F3500.
[0288] The preparation method of the inorganic silicate coating described in this embodiment comprises the following steps:
[0289] (1) At room temperature, 4 kg of cellulose, 1.6 kg of dispersant, 1 kg of stabilizer and 1.5 kg of defoamer were added to 70 kg of water and dispersed evenly at a speed of 400 r / min;
[0290] (2) Add 1 kg of antistatic agent, 60 kg of titanium dioxide, 80 kg of heavy calcium, 1 kg of toughening powder, 20 kg of sericite and 1.2 kg of anti-settling agent to the above mixture, and mix them evenly in a high-speed dispersing device at a speed of 2000 r / min for more than 20 minutes to ensure that the fineness is less than 50 μm;
[0291] (3) At a speed of 400 r / min, add 8 kg of odor-free emulsion, 0.8 kg of polyurethane leveling agent and 50 kg of modified potassium silicate to the above mixture, and mix them evenly by scraping and stirring (the stirring speed is 400 r / min). After the pH value of the system is measured to be above 11, proceed to the next step;
[0292] (4) Add 100 kg of modified potassium silicate solution and 1 kg of water-resistant agent, slowly stir and disperse for a certain period of time (stirring speed is 550 r / min, time is 60 min), and obtain the finished inorganic silicate coating.
[0293] The coating performance test described in this embodiment is shown in Table 3 below:
[0294] Table 3
[0295]
[0296]
[0297] Example 4
[0298] This embodiment provides an anti-static and fire-proof inorganic silicate coating, which differs from Example 1 only in that the modified potassium silicate provided in Preparation Example 1 is replaced by the modified potassium silicate provided in Preparation Example 3, and the antistatic agent provided in Preparation Example 7 is replaced by the antistatic agent in Preparation Example 8, and the proportions of other components are exactly the same as in Example 1.
[0299] Example 5
[0300] This embodiment provides an anti-static and fire-proof inorganic silicate coating, which differs from Example 1 only in that the modified potassium silicate provided in Preparation Example 1 is replaced by the modified potassium silicate provided in Preparation Example 4, and the antistatic agent provided in Preparation Example 7 is replaced by the antistatic agent in Preparation Example 9, and the proportions of other components are exactly the same as in Example 1.
[0301] Example 6
[0302] This embodiment provides an anti-static and fireproof inorganic silicate coating, which differs from Example 1 only in that the modified potassium silicate provided in Preparation Example 1 is replaced by the modified potassium silicate provided in Preparation Example 5, and the proportions of other components are exactly the same as those in Example 1.
[0303] Example 7
[0304] This embodiment provides an anti-static and fireproof inorganic silicate coating, which differs from Example 1 only in that the modified potassium silicate provided in Preparation Example 1 is replaced by the modified potassium silicate provided in Preparation Example 6, and the proportions of other components are exactly the same as those in Example 1.
[0305] Example 8
[0306] This embodiment provides an antistatic and fireproof inorganic silicate coating, which is different from Example 1 only in that the antistatic agent provided in Preparation Example 1 is replaced by the antistatic agent provided in Preparation Example 10, and the proportions of other components are exactly the same as those in Example 1.
[0307] Example 9
[0308] This embodiment provides an antistatic and fireproof inorganic silicate coating, which is different from Example 1 only in that the antistatic agent provided in Preparation Example 1 is replaced by the antistatic agent provided in Preparation Example 11, and the proportions of other components are exactly the same as those in Example 1.
[0309] The coating performance tests of Examples 4 to 9 are shown in Table 4 below:
[0310] Table 4
[0311]
[0312]
[0313] Comparative Example 1
[0314] This comparative example provides a coating, which is different from Example 1 only in that the antistatic agent provided in Preparation Example 7 is no longer added, and the contents of other components and the preparation method are completely consistent with those in Example 1.
[0315] The test results show that when no antistatic agent is added, the surface resistivity of the coating is very high (1.14×10 6 Ω), and the conductivity is very poor.
[0316] Comparative Example 2
[0317] This comparative example provides a coating, which is different from Example 1 only in that the modified potassium silicate provided in Preparation Example 1 is replaced by conventional potassium silicate of equal mass, and the contents of other components and the preparation method are exactly the same as those in Example 1.
[0318] The fire retardant performance test of the coating in this comparative example is shown in Table 5 below:
[0319] Table 5
[0320]
[0321] Comparative Example 3
[0322] This comparative example provides a coating, which differs from Example 1 only in that the organic fluorine resin modified potassium silicate is changed to a composite of potassium silicate and acrylic resin, that is, the modified potassium silicate provided in Preparation Example 1 is replaced by the modified potassium silicate provided in Comparative Preparation Example 1, and the contents of other components and the preparation method are exactly the same as those in Example 1.
[0323] The fire retardant performance test of the coating in this comparative example is shown in Table 6 below:
[0324] Table 6
[0325]
[0326] It can be seen from the experimental results of Example 1 and Comparative Examples 2 to 5 that the fire retardant performance of the inorganic coating obtained in the absence of organic fluorine resin is greatly weakened compared with the examples.
[0327] Comparative Example 4
[0328] This comparative example provides a coating, which is different from Example 1 only in that the antistatic agent provided in Preparation Example 7 is replaced by the antistatic agent provided in Comparative Preparation Example 2, and the contents of other components and the preparation method are completely consistent with those in Example 1.
[0329] The test results show that when the antistatic agent polyaniline / conductive sericite composite material is changed to conventional conductive sericite, the surface resistivity of the coating is higher (4.14×10 5 Ω), poor electrical conductivity.
[0330] Comparative Example 5
[0331] This comparative example provides a coating, which is different from Example 1 only in that the antistatic agent provided in Preparation Example 7 is replaced by the antistatic agent provided in Comparative Preparation Example 3, and the contents of other components and the preparation method are completely consistent with those in Example 1.
[0332] The test results show that when the antistatic agent polyaniline / conductive sericite composite material is changed to a conventional sericite surface directly coated with a polyaniline layer without a tin oxide-antimony oxide composite layer, the surface resistivity of the coating is higher (7.26×10 5 Ω), poor electrical conductivity.
[0333] Comparative Example 6
[0334] This comparative example provides a coating, which is different from Example 1 only in that the stabilizer silica sol is replaced by a stabilizer aluminum sol of equal mass, and the contents of other components and the preparation method are completely consistent with those of Example 1.
[0335] Comparative Example 7
[0336] This comparative example provides a coating, which is different from Example 1 only in that the toughening agent is replaced by an equal mass of toughening agent dibutyl phthalate, and the contents of other components and the preparation method are completely consistent with those in Example 1.
[0337] Comparative Example 8
[0338] This comparative example provides a coating, which is different from Example 1 only in that sericite is replaced by kaolin of equal mass, and the contents of other components and the preparation method are exactly the same as those in Example 1.
[0339] Comparative Example 9
[0340] This comparative example provides a coating, which is different from Example 1 only in that the anti-settling agent water-based polyamide is replaced by an anti-settling agent polyolefin wax of equal mass, and the contents of other components and the preparation method are completely consistent with those of Example 1.
[0341] Comparative Example 10
[0342] This comparative example provides a coating, which is different from Example 1 only in that the water-resistant agent polyethylene wax emulsion is replaced by an equal mass of water-resistant agent polysiloxane powder, and the contents of other components and the preparation method are completely consistent with those in Example 1.
[0343] The fire retardant performance tests of the coatings described in Comparative Examples 6 to 10 are shown in Table 7 below:
[0344] Table 7
[0345]
[0346]
[0347] As shown in the above table, the stabilizer, toughening powder, sericite, anti-settling agent and water-resistant agent in Example 1 were replaced with other types of reagents. It was found that the performance of the resulting coating (including data such as benzene content, state in the container and washability) was poor.
[0348] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An antistatic and fireproof inorganic silicate coating, characterized in that: The raw materials for preparing the antistatic and fireproof inorganic silicate coating include, by weight: 25-40 parts of modified potassium silicate, 35-70 parts of filler, 0.2-0.8 parts of cellulose, 0.1-0.5 parts of antistatic agent, 1-20 parts of functional additive, and 15-23 parts of water; The modified potassium silicate comprises a potassium silicate core and an organic fluorine shell layer coated on the surface of the potassium silicate core; The antistatic agent comprises conductive sericite and a polyaniline layer deposited on the surface of the conductive sericite.
2. The antistatic and fireproof inorganic silicate coating according to claim 1, characterized in that: The raw materials for preparing the modified potassium silicate include, by weight: 2-4 parts of acrylate monomer, 2-4 parts of fluorine-containing vinyl monomer, 15-30 parts of alkaline potassium silicate sol, 0.03-0.1 parts of organosilicon coupling agent, 0.1-1 parts of initiator, 1-10 parts of solvent; Preferably, the acrylic acid ester monomer is butyl acrylate; Preferably, the fluorine-containing vinyl monomer is 1,1-difluoroethylene and / or trifluoroethylene; Preferably, the alkaline potassium silicate sol has a pH of 9 to 10 and a solid content of 20 to 40 wt %; Preferably, the organic silicon coupling agent is γ-methacryloxypropyltrimethoxysilane; Preferably, the initiator is dibenzoyl peroxide; Preferably, the solvent is ethylene glycol monobutyl ether.
3. The antistatic and fireproof inorganic silicate coating according to claim 1 or 2, characterized in that: The modified potassium silicate is prepared by the following steps: After dissolving the first part of the initiator in the solvent, heating to 80-120° C., a raw material solution 1 is obtained; Mixing an acrylic acid ester monomer, a fluorine-containing vinyl monomer and a second part of an initiator to obtain a second raw material solution, and dripping the second raw material solution into the first raw material solution; After the second raw material solution has been added for 10 to 20 minutes, the mixed solution of alkaline potassium silicate sol and organosilicon coupling agent is added to the first raw material solution simultaneously, and the adding time is controlled to be 1 to 3 hours; After the dropwise addition is completed, the remaining initiator is added to the mixed solution, and a constant temperature reaction is carried out at 105 to 115° C. for 0.5 to 1.5 hours to obtain the modified potassium silicate; Preferably, the mass ratio of the first part of initiator, the second part of initiator and the remaining initiator is 2:1:1; Preferably, after the isothermal reaction is completed, the following steps are further included: reducing the temperature of the reaction solution after the isothermal reaction to below 45° C., adjusting the pH of the solution to 7-8, and obtaining the modified potassium silicate.
4. The antistatic and fireproof inorganic silicate coating according to claim 1, characterized in that: The raw materials for preparing the antistatic agent include, by weight: 4 to 6 parts of conductive sericite, 0.4 to 0.6 parts of p-phenylenediamine, 0.1 to 0.12 parts of phosphoric acid, and 4 to 6 parts of initiator; Preferably, the initiator is dibenzoyl peroxide; Preferably, the conductive sericite comprises sericite and a conductive oxide layer deposited on the surface of the sericite; Preferably, the raw materials for preparing the conductive sericite include, by weight: 8-11 parts of tin salt, 1-3 parts of antimony salt, 18-23 parts of sericite, 30-35 parts of acid solution, 4-7 parts of sodium tripolyphosphate solution, 30-40 parts of alkali solution; Preferably, the tin salt is tin tetrachloride; Preferably, the antimony salt is antimony trichloride; Preferably, the acid solution is a 10-20wt% hydrochloric acid aqueous solution; Preferably, the sodium tripolyphosphate solution is a 20-40wt% sodium tripolyphosphate aqueous solution; Preferably, the alkali solution is a 10-20 wt % sodium hydroxide aqueous solution.
5. The antistatic and fireproof inorganic silicate coating according to claim 1 or 4, characterized in that: The antistatic agent is prepared by the following steps: Dispersing sericite in water to obtain a sericite suspension; mixing tin salt, antimony salt and acid solution to obtain a mixed solution; simultaneously dropping the mixed solution and alkali solution into the sericite suspension to react at 10-40° C. for 0.5-1.5 hours to obtain a first reaction solution; dropping sodium tripolyphosphate solution into the first reaction solution, stirring at 10-40° C. for 0.5-1.5 hours, filtering, washing and drying in sequence, and calcining at 750-850° C. for 4-6 hours to obtain the conductive sericite; Dispersing conductive sericite in water to obtain a conductive sericite dispersion; adding p-phenylenediamine and phosphoric acid to the conductive sericite dispersion, stirring at 10 to 40° C. for 0.5 to 1.5 hours to obtain a mixed solution; dissolving an initiator in water to obtain an initiator solution; dropping the initiator solution into the mixed solution, stirring at 10 to 40° C. for 6 to 18 hours, and then filtering, washing, drying, crushing and grinding to obtain the antistatic agent.
6. The antistatic and fireproof inorganic silicate coating according to claim 1, characterized in that: The filler includes any one of titanium dioxide, heavy calcium or sericite, or a combination of at least two thereof; Preferably, the filler comprises, by weight: 20 to 30 parts of titanium dioxide, 15 to 30 parts of heavy calcium, and 3 to 10 parts of sericite; Preferably, the mesh size of the heavy calcium is 800-1250 mesh; Preferably, the cellulose is a hydrophobic hydroxyalkyl modified cellulose, preferably a hydrophobic hydroxyethyl modified cellulose; Preferably, the cellulose has a hydroxyl content of 18-23% and an ethyl content of 5-7%; Preferably, the cellulose comprises any one of 250HRR, 250HHBR, HE10K, M-100, 30000H or HS10, or a combination of at least two thereof; Preferably, the functional additive includes any one or a combination of at least two of a dispersant, a stabilizer, a defoamer, a toughening agent, an anti-settling agent, a deodorizing emulsion, a leveling agent or a water-resistant agent; Preferably, the functional additives include, by weight: 0.2-0.6 parts of dispersant, 0.1-1 parts of stabilizer, 0.1-1 parts of defoamer, 0.1-1 parts of toughening agent, 0.1-1 parts of anti-settling agent, 1-8 parts of odor-free emulsion, 0.1-1 parts of leveling agent and 0.1-1 parts of water-resistant agent; Preferably, the dispersant includes any one of a sodium salt dispersant, an ammonium salt dispersant or a high molecular polymer dispersant, or a combination of at least two thereof; Preferably, the stabilizer is silica sol; Preferably, the defoamer includes any one of a mineral oil defoamer, a silicone defoamer, a polyether defoamer or a polyether-modified silicone defoamer, or a combination of at least two thereof; Preferably, the toughening agent is vinyl acetate-ethylene copolymer emulsion; Preferably, the anti-settling agent is water-based polyamide; Preferably, the deodorizing emulsion comprises any one or a combination of at least two of styrene acrylic emulsion, silicone acrylic emulsion, acrylate emulsion, polyvinyl acetate emulsion, ethylene vinyl acetate emulsion or ethylene acrylate emulsion; Preferably, the leveling agent is a polyurethane leveling agent; Preferably, the water-resistant agent is polyethylene wax emulsion.
7. A method for preparing an antistatic and fireproof inorganic silicate coating according to any one of claims 1 to 6, characterized in that: The preparation method comprises: Modified potassium silicate, filler, cellulose, antistatic agent and functional additive are dispersed in water according to a proportion to obtain the antistatic and fireproof inorganic silicate coating.
8. The method for preparing the antistatic and fireproof inorganic silicate coating according to claim 7, characterized in that: The preparation method specifically comprises the following steps: (1) adding cellulose, a dispersant, a stabilizer and a defoamer into water for a first dispersion to obtain a mixed solution 1; (2) adding a filler, an antistatic agent, a toughening agent and an anti-settling agent to the mixed solution 1, and performing a second dispersion to obtain a mixed solution 2; (3) adding a deodorizing emulsion, a leveling agent and a portion of modified potassium silicate to the mixed solution 2, scraping and stirring to obtain a mixed solution 3; (4) Adding a water-resistant agent and the remaining modified potassium silicate to the mixed solution 3, stirring the mixture, and obtaining the antistatic and fireproof inorganic silicate coating.
9. The method for preparing the antistatic and fireproof inorganic silicate coating according to claim 8, characterized in that: In step (1), the rotation speed of the first dispersion is 300 to 500 r / min; Preferably, in step (2), the rotation speed of the second dispersion is 1500-2500 r / min, and the time of the second dispersion is more than 20 min; Preferably, in step (2), the fineness of the particles in the second mixed solution is less than 50 μm; Preferably, in step (3), the mass of the modified potassium silicate accounts for 20-40% of the total mass of the modified potassium silicate; Preferably, in step (3), the stirring speed is 300 to 500 r / min; Preferably, in step (3), the pH of the mixed solution 3 is above 11; Preferably, in step (4), the stirring speed is 500-800 r / min.
10. Use of the antistatic and fireproof inorganic silicate coating according to any one of claims 1 to 6 in the protection of building facilities in the northwest region.