Reflective heat-insulation real stone paint as well as preparation method and application thereof
By using core-shell thermal insulation emulsion and functional raw materials such as reflective thermal insulation coating stones and rock flakes, the storage stability and construction problems of existing reflective thermal insulation real stone paint are solved, and higher thermal insulation effect and lightweight Qualification meets the application requirements of energy-saving buildings.
Patent Information
- Application Number
- CN202411108492.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing reflective heat-insulating real stone paint has poor storage stability, poor construction properties, difficult to meet the standards for medium and low brightness, high construction consumption, and is not conducive to low-carbon sustainable development.
Core-shell thermal insulation emulsion is used to replace the traditional functional filler hollow glass microbeads, and reflective insulation cover stone and reflective insulation rock sheets instead of natural colored sand. Combining stone powder and pigment powder, it forms a reflective insulation with higher insulation effect. Real stone paint.
It significantly improves the reflective insulation effect and storage stability of real stone paint, reduces construction consumption, achieves lightweight and color diversity, and meets the needs of thermal insulation materials in the energy-saving construction field.
Smart Images

Figure BDA0004991501500000071 
Figure BDA0004991501500000081 
Figure BDA0004991501500000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a reflective heat-insulating real stone paint and a preparation method and application thereof. Background Art
[0002] Energy-saving buildings are a new type of building that is energy-saving, environmentally friendly and comfortable. Improving the thermal insulation effect of living space is an important part of developing energy-saving buildings and is the key to improving energy efficiency and enhancing building comfort and functionality. When achieving thermal insulation functions, the selection of thermal insulation materials, the layout of the thermal insulation system and the design of the thermal insulation system are all crucial.
[0003] Reflective heat-insulating paint refers to a functional paint with high solar reflectance and high hemispherical reflectivity, which has the functions of reflecting sunlight and heat insulation. Reflective heat-insulating real stone paint is a functional paint with strong decorative properties commonly used for exterior walls. The reflective heat-insulating real stone paint on the market currently mainly uses synthetic resin as the film-forming material, and is formulated with reflective heat-insulating functional fillers, pigments, additives, natural sand and other raw materials. It mainly achieves high reflective heat-insulating effects by adding functional fillers such as hollow glass microspheres or hollow ceramic microspheres. This type of reflective heat-insulating real stone paint has the disadvantages of poor storage stability, poor construction performance, difficulty in meeting the standards for medium and low brightness, high construction consumption, and is not conducive to low-carbon sustainable development. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a reflective heat-insulating real stone paint; the second purpose of the present invention is to provide a preparation method of the reflective heat-insulating real stone paint; the third purpose of the present invention is to provide an application of the reflective heat-insulating real stone paint.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a reflective heat-insulating real stone paint, comprising the following preparation raw materials: base material, reflective heat-insulating coated stone, reflective heat-insulating rock flakes, stone powder and pigment powder;
[0007] The raw materials for preparing the reflective heat-insulating coated stone include coating liquid and stone; the coating liquid includes heat-insulating emulsion, acrylic emulsion and film-forming aid;
[0008] The raw materials for preparing the reflective heat-insulating rock sheet include heat-insulating emulsion, elastic pure acrylic emulsion and expanded pearlite powder;
[0009] The raw materials for preparing the base material include heat insulation emulsion.
[0010] Preferably, the thermal insulation emulsion is a core-shell emulsion; further preferably, the thermal insulation emulsion includes at least one of a core-shell silicone-acrylic emulsion and a core-shell acrylic emulsion.
[0011] Preferably, the particle size of the core-shell emulsion is 1000-2000 nm, and the inner core particle size is 300-600 nm.
[0012] Preferably, the solid content of the core-shell emulsion is 40-55 wt %.
[0013] Preferably, the core-shell acrylic emulsion is prepared by a method comprising the following steps:
[0014] 1) reacting an emulsifier, an unsaturated acid, an olefin monomer, an initiator, a siloxane compound with an active group and water to obtain a seed emulsion;
[0015] 2) reacting an emulsifier, an unsaturated acid, an olefin monomer, an initiator, a seed emulsion and water to obtain the core-shell acrylic emulsion.
[0016] Preferably, the emulsifier is selected from at least one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, fatty alcohol polyoxyethylene ether, polyoxyethylene alkyl ester, and sodium cetyl betaine.
[0017] Preferably, the unsaturated acid is selected from at least one of acrylic acid, methacrylic acid, itaconic acid and fumaric acid.
[0018] Preferably, the olefin monomer is selected from at least one of styrene, methyl methacrylate, butyl acrylate, acrylonitrile and isooctyl acrylate.
[0019] Preferably, the initiator is selected from at least one of sodium persulfate, ammonium persulfate and potassium persulfate.
[0020] Preferably, the siloxane compound with active groups is prepared by a method comprising the following steps: methacryloxypropyl alkoxysilane reacts with alkyl silicate to obtain a siloxane compound with active groups; wherein the methacryloxypropyl alkoxysilane is selected from at least one of γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl triethoxysilane or γ-methacryloxypropyl methyldimethoxysilane; and the alkyl silicate is selected from at least one of methyl orthosilicate and ethyl orthosilicate.
[0021] Specifically, the present invention replaces the traditional functional filler hollow glass microspheres with a thermal insulation emulsion with a core-shell structure. The hollow volume of the thermal insulation emulsion is 10-20 times the hollow volume of the traditional hollow glass microspheres, which can effectively reduce the thermal conductivity coefficient, provide better thermal insulation effect, and solve the problems of poor storage stability and poor construction performance of existing real stone paint.
[0022] Preferably, the reflective heat-insulating real stone paint comprises the following raw materials, measured by mass: 20-30 parts of base material, 60-80 parts of reflective heat-insulating coated stone, 0.1-2 parts of reflective heat-insulating rock flakes, 3-6 parts of stone powder, and 0.1-2 parts of pigment powder.
[0023] Preferably, the raw materials for preparing the reflective heat-insulating real stone paint also include a wetting agent and a thickener.
[0024] Preferably, the wetting agent comprises a fatty alcohol polyether wetting agent; preferably at least one of Clariant Genapol X 080, Clariant Genapol PF 20, San Nopco SN-WET 966, and San Nopco SN-WET 126.
[0025] Preferably, the thickener includes a hydrophobically modified alkali-swellable thickener; preferably, Yale Shun TT-615, Wanhua A801, Wanhua At least one of TA66.
[0026] Preferably, the reflective heat-insulating real stone paint is prepared from the following raw materials, measured by mass: 20-30 parts of base material, 60-80 parts of reflective heat-insulating coated stone, 0.1-2 parts of reflective heat-insulating rock flakes, 3-6 parts of stone powder, 0.1-2 parts of pigment powder, 0.1-1 parts of wetting agent, and 0.1-2 parts of thickener.
[0027] Preferably, the base material comprises the following raw materials, measured by mass: 40-60 parts of thermal insulation emulsion, 30-50 parts of water, 0.1-1 part of cellulose, 0.1-1 part of pH regulator, 0.1-3 parts of film-forming aid, 0.1-1 part of antifreeze agent, 0.1-1 part of defoaming agent, and 0.1-1 part of preservative.
[0028] Preferably, the base material is prepared by a method comprising the following steps:
[0029] Water and cellulose are mixed, and stirred and dispersed at 500-700 rpm for 5-10 minutes, and a pH regulator, a film-forming aid, an antifreeze agent, a heat-insulating emulsion, a defoaming agent and a preservative are added in sequence, and stirring is continued for 5-10 minutes to obtain the base material.
[0030] Preferably, the reflective insulation coated stone comprises the following raw materials in parts by mass: 5-15 parts of coating liquid and 95-105 parts of stone; the coating liquid comprises the following raw materials in parts by mass: 25-35 parts of insulation emulsion, 55-65 parts of acrylic emulsion and 1-2 parts of film-forming aid.
[0031] Preferably, the raw materials for preparing the coating liquid also include inorganic reflective thermal insulation color paste; the type and amount of the inorganic reflective thermal insulation color paste are adjusted according to the required color; further preferably, the inorganic reflective thermal insulation color paste includes Clariant inorganic reflective thermal insulation color paste.
[0032] Preferably, the stone material comprises expanded perlite. Expanded perlite itself has a multi-microporous structure, low density characteristics and excellent heat insulation capacity. After being coated with coating liquid, its reflective heat insulation effect can be further improved.
[0033] Preferably, the acrylic emulsion is selected from at least one of Budford RS-9977A, Budford RS-998A, and Budford RS-992A.
[0034] Preferably, the particle size of the reflective insulation coated stone is selected from at least one of 40-80 mesh, 80-120 mesh, and 120-180 mesh.
[0035] Preferably, the reflective heat-insulating coated stone includes 15-25 parts of 40-80 mesh reflective heat-insulating coated stone, 35-45 parts of 80-120 mesh reflective heat-insulating coated stone, and 35-45 parts of 120-180 mesh reflective heat-insulating coated stone by weight. The smaller the particle size of the reflective heat-insulating coated stone, the more conducive to reducing construction consumption and achieving lightweight, but using only 120-180 mesh reflective heat-insulating coated stone will easily lead to unqualified initial crack resistance.
[0036] Specifically, the present invention uses reflective insulation coated stone to replace the 40-80 mesh, 80-120 mesh, and 120-180 mesh natural colored sand in the existing real stone paint, which can not only improve the reflective insulation effect of the real stone paint and solve the problem of unqualified medium and low brightness, but also realize the color diversity and customization of the real stone paint and improve the lightweight effect of the real stone paint.
[0037] Preferably, the reflective heat-insulating coated stone is prepared by a method comprising the following steps:
[0038] 1) mixing a heat-insulating emulsion, an acrylic emulsion, a film-forming aid and an inorganic reflective heat-insulating color paste to obtain a coating liquid;
[0039] 2) Add stones to the reaction kettle, set the speed to 50-100 rpm, turn on the heating to raise the temperature to 70-90°C, spray the coating liquid, stir for 5-10 minutes, and dry for 5-10 minutes to obtain the reflective heat-insulating coated stone.
[0040] Preferably, the reflective heat-insulating rock sheet comprises the following raw materials, measured by mass: 35-45 parts of heat-insulating emulsion, 35-45 parts of elastic pure acrylic emulsion, and 15-25 parts of expanded perlite powder.
[0041] Preferably, the raw materials for preparing the reflective thermal insulation rock sheet also include inorganic reflective thermal insulation color paste; the type and amount of the inorganic reflective thermal insulation color paste are adjusted according to the required color; further preferably, the inorganic reflective thermal insulation color paste includes Clariant inorganic reflective thermal insulation color paste.
[0042] Preferably, the reflective heat-insulating rock sheet is made by a method comprising the following steps:
[0043] The heat-insulating emulsion is mixed with the elastic pure acrylic emulsion to obtain a composite emulsion, and expanded pearlite powder and inorganic reflective heat-insulating color paste are added, and the reflective heat-insulating rock sheet is obtained by thermoplastic molding.
[0044] Preferably, the thickness of the reflective heat-insulating rock sheet is 0.01-0.1 mm.
[0045] Preferably, the particle size of the reflective insulation rock piece is 0.3-1.5 mm.
[0046] Specifically, the reflective heat-insulating rock sheet used in the present invention is light and thin, and is used to replace the 10-40 mesh natural colored sand used in existing real stone paint. While ensuring its embellishment effect, it can also improve the phenomenon of rebounding and falling sand during the construction of natural colored sand, and assist in improving the reflective heat-insulating effect and lightweight effect of real stone paint.
[0047] Preferably, the stone powder comprises calcite powder.
[0048] Preferably, the particle size of the stone powder is 180-250 mesh; the stone powder is preferably ultrafine calcite powder CC-200 produced by Guangdong Fujian Building Materials (Jiaoling) Refining Co., Ltd.
[0049] Preferably, the particle size of the pigment powder is 200-300 meshes; the pigment powder is ground from natural colored ore, preferably the natural color powder from Nanzhao County Jiacheng Mining Co., Ltd.
[0050] Specifically, the stone powder and pigment powder used in the present invention have excellent dispersibility and weather resistance, can provide excellent hiding power and color matching, reduce the use of natural colored sand, reduce the construction consumption of real stone paint, and achieve lightweight.
[0051] Preferably, the cellulose comprises hydrophobically modified hydroxyethyl cellulose ether; preferably at least one of Ashland 250HBR, Ashland 250H4BR, and Ashland HE-10K.
[0052] Preferably, the pH adjuster includes at least one of diethanolamine, butyl diethylenediamine, 2-amino-2-methyl-1-propanol, and 2-amino-2-ethyl-1,3-propanediol; preferably, it is Dow's multifunctional additive APM-95.
[0053] Preferably, the antifreeze comprises an alcohol antifreeze; further preferably, the antifreeze comprises at least one of ethylene glycol, propylene glycol and polyethylene glycol.
[0054] Preferably, the defoaming agent includes at least one of polysiloxane, polyether-modified dimethylsiloxane, and polymer composite mineral oil; preferably at least one of BASF FoamstarST 2410AG (A10) and BASF Foamaster MO NXZ.
[0055] Preferably, the preservative includes at least one of 5-chloro-2-methylisothiazoline-3-one, 2-methyl-4-isothiazoline-3-one, and 1,2-benzisothiazolin-3-one; preferably at least one of Dow BIOBAN CM 14 and Dow BT NV2.
[0056] Preferably, the film-forming aid includes an alcohol ester film-forming aid; preferably Eastman TEXANOL ester alcohol 12, Tairun -16 hexadecanediol, Dow COASOL 290 or at least one of them.
[0057] Preferably, the reflective heat-insulating real stone paint has a viscosity of 90-130 dps at 25°C.
[0058] The second aspect of the present invention provides a method for preparing the reflective heat-insulating real stone paint according to the first aspect of the present invention, comprising the following steps:
[0059] The prepared raw materials are mixed to obtain the reflective heat-insulating real stone paint.
[0060] Preferably, the method specifically comprises the following steps:
[0061] Add the base material into the reaction kettle, start stirring at a speed of 500-800rpm, add the wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in sequence, stir for 5min-10min, add the thickener, and obtain the reflective insulation real stone paint.
[0062] Preferably, during the preparation of the reflective heat-insulating real stone paint, the rotation speed can be appropriately increased as the viscosity increases.
[0063] The third aspect of the present invention provides the application of the reflective heat-insulating real stone paint described in the first aspect of the present invention in the field of energy-saving buildings.
[0064] Compared with the prior art, the present invention has the following beneficial effects:
[0065] 1) The reflective heat-insulating real stone paint provided by the present invention uses a heat-insulating emulsion to modify stones and rock flakes, thereby increasing the types of raw materials with heat-insulating functions in the preparation of real stone paint; the reflective heat-insulating coated stones are used to replace the 40-80 mesh, 80-120 mesh, and 120-180 mesh natural colored sand in the existing real stone paint, thereby effectively improving the reflective heat-insulating effect of the real stone paint, solving the problem of unqualified medium and low brightness, increasing the color diversity and customization of the real stone paint, and achieving lightweight; the reflective heat-insulating rock flakes are used to replace the existing real stone paint The 10-40 mesh natural colored sand is used to embellish the natural colored sand. While ensuring the embellishment effect, it improves the phenomenon of rebounding and falling sand during the construction of the natural colored sand, and further realizes the lightweight while improving the reflective heat insulation effect of the real stone paint. The core-shell type heat insulation emulsion in the base material replaces the traditional functional filler hollow glass beads, and the hollow volume is 10-20 times that of the hollow glass beads, which makes the reflective heat insulation real stone paint have better storage stability, construction performance and heat insulation effect; the synergistic effect of various heat insulation functional raw materials significantly improves the comprehensive performance of the real stone paint.
[0066] 2) The reflective heat-insulating real stone paint provided by the present invention is added with stone powder and pigment powder, both of which have excellent dispersibility and weather resistance, can provide excellent hiding and color matching properties, reduce the use of natural colored sand, reduce the construction consumption of real stone paint, and achieve lightweight.
[0067] 3) The reflective heat-insulating real stone paint provided by the present invention has good storage stability, good heat-insulating effect, low construction consumption, light weight, and a simple preparation method, and can meet the application requirements of heat-insulating materials in the field of energy-saving buildings. DETAILED DESCRIPTION
[0068] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0069] 1. "Parts" in the following examples and comparative examples refer to "parts by mass" unless otherwise specified.
[0070] 2. The raw materials for preparing the reflective heat-insulating coated stones in the following examples and comparative examples are: 10 parts of coating liquid and 100 parts of stone. The coating liquid is composed of 30 parts of heat-insulating emulsion, 60 parts of acrylic emulsion, 1.5 parts of film-forming aid and inorganic reflective heat-insulating color paste. The stone is composed of 20 parts of 40-80 mesh natural expanded perlite, 40 parts of 80-120 mesh natural expanded perlite and 120-180 mesh natural expanded perlite. The acrylic emulsion is Badford RS-9977A, the film-forming aid is Eastman TEXANOL ester alcohol twelve, and the inorganic reflective heat-insulating color paste is Clariant inorganic reflective heat-insulating color paste.
[0071] The preparation method is as follows: heat insulation emulsion, acrylic emulsion, film-forming aid and inorganic reflective heat insulation color paste are mixed to obtain coating liquid, stone is added to the reaction kettle, the speed is set to 80rpm, heating is turned on to raise the temperature to 80℃, coating liquid is sprayed, stirred for 8min, dried for 8min, and reflective heat insulation coated stone is obtained. The particle sizes of reflective heat insulation coated stone include 40-80 mesh, 80-120 mesh and 120-180 mesh.
[0072] 3. The raw materials for preparing the reflective thermal insulation rock sheets in the following examples and comparative examples are: 20 parts of inorganic expanded perlite powder, 40 parts of thermal insulation emulsion, 40 parts of elastic pure acrylic emulsion and Clariant inorganic reflective thermal insulation color paste.
[0073] The preparation method is as follows: heat insulation emulsion is mixed with elastic pure acrylic emulsion to obtain composite emulsion, expanded pearlite powder and inorganic reflective heat insulation color paste are added, and thermoplastic molding is performed to obtain reflective heat insulation rock sheet. The thickness of the reflective heat insulation rock sheet is 0.05mm and the particle size is 1.0mm.
[0074] 4. The core-shell thermal insulation acrylic emulsions in the following examples and comparative examples are prepared by the following steps:
[0075] S1, first take 100g of ethyl silicate and put it into 50g of deionized water, stir evenly, add 0.01-0.05g of glacial acetic acid during stirring, raise the temperature to 40-50°C, continue stirring for 5min, then drop 10g of γ-methacryloxypropyltriethoxysilane monomer into the water, react for 30min, cool down, add 0.1% (w / v) of tetrahydroxypropylethylenediamine as a stabilizer in the mixed solution, and finally filter to obtain a siloxane compound with an active group;
[0076] S2, dispersing the emulsifier sodium dodecylbenzene sulfonate (DS-4) in deionized water, slowly adding the olefin monomer methyl methacrylate (MMA) and the unsaturated acid methacrylic acid (MAA) into the water under stirring, dispersing at a speed of 600rpm for 10min, preparing the pre-emulsion for dropwise reaction; mixing sodium persulfate and water evenly, and setting aside as a titration initiator; preparing a reaction flask, adding a certain amount of water and heating it to 83-89°C, adding about 2% of the pre-emulsion, and adding a part of the sodium persulfate aqueous solution, keeping the temperature at 83-85°C for 15min, and showing a blue fluorescent state; continuing to dropwisely add the remaining pre-emulsion and the remaining sodium persulfate aqueous solution at 83-85°C for reaction at a uniform speed, stirring at a uniform speed for 4h until the reaction is formed into an emulsion; putting the previously treated silane into the reactor at one time, washing it with water, controlling the temperature to 83-85°C for insulation reaction for 2h, finally cooling it down, filtering the emulsion, and obtaining an acrylic acid seed emulsion;
[0077] S3, adding acrylic seed emulsion to water, heating to 90-93°C, adding sodium persulfate, dripping emulsion composed of sodium dodecylbenzene sulfonate (DS-4), styrene (ST), methyl methacrylate (MMA), allyl methacrylate (AMA), methacrylic acid (MAA) and water and sodium persulfate, the dripping time is 150min, adding ammonia water when dripping 45% emulsion, reacting for 5min, and continuing to drip; cooling to 80-83°C after the dripping reaction, post-processing reaction with tert-butyl hydroperoxide and ascorbic acid, keeping warm for 20min; cooling to below 50°C and discharging to obtain core-shell type thermal insulation acrylic emulsion. The particle size of the emulsion is 1700nm, the inner core particle size is 550nm, and the solid content is 40wt%.
[0078] The core-shell type heat-insulating acrylic emulsion is used for preparing reflective heat-insulating coated stone and reflective heat-insulating rock slices.
[0079] Example 1
[0080] This embodiment provides a reflective heat-insulating real stone paint, and the raw materials for preparation are shown in Table 1:
[0081] Table 1 Raw materials for preparing reflective heat-insulating real stone paint in Example 1
[0082]
[0083] The reflective heat-insulating real stone paint is prepared by the following steps:
[0084] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0085] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0086] Example 2
[0087] This embodiment provides a reflective heat-insulating real stone paint, and the raw materials for preparation are shown in Table 2:
[0088] Table 2 Raw materials for preparing reflective heat-insulating real stone paint in Example 2
[0089]
[0090] The reflective heat-insulating real stone paint is prepared by the following steps:
[0091] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0092] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0093] Example 3
[0094] This embodiment provides a reflective heat-insulating real stone paint, and the raw materials for preparation are shown in Table 3:
[0095] Table 3 Raw materials for preparing reflective heat-insulating real stone paint in Example 3
[0096]
[0097] The reflective heat-insulating real stone paint is prepared by the following steps:
[0098] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0099] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0100] Example 4
[0101] This embodiment provides a reflective heat-insulating real stone paint, and the raw materials for preparation are shown in Table 4:
[0102] Table 4 Raw materials for preparing reflective heat-insulating real stone paint in Example 4
[0103]
[0104]
[0105] The reflective heat-insulating real stone paint is prepared by the following steps:
[0106] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0107] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0108] Comparative Example 1
[0109] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 5:
[0110] Table 5 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 1
[0111]
[0112]
[0113] The reflective heat-insulating real stone paint is prepared by the following steps:
[0114] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, ordinary silicone-acrylic emulsion, defoamer and preservative are sequentially added, and stirring is continued for 8 minutes to obtain a base material;
[0115] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0116] Comparative Example 2
[0117] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 6:
[0118] Table 6 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 2
[0119]
[0120]
[0121] The reflective heat-insulating real stone paint is prepared by the following steps:
[0122] 1) Water and cellulose were sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, hollow glass microspheres, film-forming aid, antifreeze agent, ordinary silicone-acrylic emulsion, defoamer and preservative were sequentially added, and stirred for 8 minutes to obtain a base material;
[0123] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and reflective insulation rock flakes in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0124] Comparative Example 3
[0125] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 7:
[0126] Table 7 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 3
[0127]
[0128]
[0129] The reflective heat-insulating real stone paint is prepared by the following steps:
[0130] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0131] 2) Add the base material into the reactor, start stirring at 700 rpm, add reflective insulation coated stone and reflective insulation rock flakes in turn, as the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100 dps, and obtain reflective insulation real stone paint.
[0132] Comparative Example 4
[0133] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 8:
[0134] Table 8 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 4
[0135]
[0136]
[0137] The reflective heat-insulating real stone paint is prepared by the following steps:
[0138] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0139] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, reflective insulation coated stone and natural colored sand in turn. As the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0140] Comparative Example 5
[0141] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 9:
[0142] Table 9 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 5
[0143]
[0144] The reflective heat-insulating real stone paint is prepared by the following steps:
[0145] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0146] 2) Add the base material into the reactor, start stirring at 700rpm, add wetting agent, stone powder, pigment powder, natural colored sand and reflective insulation rock flakes in turn, as the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add thickener to adjust the viscosity to 100dps, and obtain reflective insulation real stone paint.
[0147] Comparative Example 6
[0148] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 10:
[0149] Table 10 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 6
[0150]
[0151] The reflective heat-insulating real stone paint is prepared by the following steps:
[0152] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, heat insulation emulsion, defoamer and preservative are sequentially added, and stirred for 8 minutes to obtain a base material;
[0153] Add the base material into the reactor, start stirring at 700rpm, add natural colored sand, as the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add a thickener to adjust the viscosity to 100dps, and obtain reflective heat-insulating real stone paint.
[0154] Comparative Example 7
[0155] This comparative example provides a reflective heat-insulating real stone paint, and the raw materials for its preparation are shown in Table 11:
[0156] Table 11 Raw materials for preparing reflective heat-insulating real stone paint in comparative example 7
[0157]
[0158] The reflective heat-insulating real stone paint is prepared by the following steps:
[0159] 1) Water and cellulose are sequentially added into a reaction kettle, stirred at 600 rpm, dispersed for 8 minutes, and then pH regulator, film-forming aid, antifreeze agent, ordinary silicone-acrylic emulsion, defoamer and preservative are sequentially added, and stirring is continued for 8 minutes to obtain a base material;
[0160] 2) Add the base material into the reactor, start stirring at 700 rpm, add natural colored sand, as the viscosity increases, increase the speed appropriately, stir evenly for 8 minutes, add a thickener to adjust the viscosity to 100 dps, and obtain reflective heat-insulating real stone paint.
[0161] Performance Testing
[0162] The basic properties and reflective heat insulation effects of the reflective heat insulation real stone paint in test examples 1-4 and comparative examples 1-7 are tested, wherein the reflective heat insulation effect test indicators include solar reflectance, near-infrared reflectance, hemispherical emissivity and thermal conductivity, and the test methods and standards refer to GB / T 25261-2018 "Reflective Heat Insulation Coatings for Buildings"; basic performance test indicators include surface drying time, initial drying crack resistance, low temperature stability, thermal storage stability, construction performance, water absorption, water resistance, alkali resistance, coating temperature change resistance, stain resistance and bonding strength, and the test methods and standard limits refer to JG / T 24-2018 "Synthetic Resin Emulsion Sand Wall Architectural Coatings".
[0163] In addition, in order to further evaluate the lightweight effect of reflective heat-insulating real stone paint, its consumption was evaluated using the real stone paint hiding power index.
[0164] The hiding power test method is: take a small white card with a black cross dividing seam, use a stainless steel frame of different thicknesses to apply the real stone paint on the small white card with a scraper, and then visually inspect it after it dries. It is qualified if no black cross dividing seam can be seen. The real stone paint consumption is evaluated based on the hiding power, that is, the real stone paint consumption = real stone paint density * stainless steel frame volume / stainless steel frame area.
[0165] The test method for sand drop rate is: the real stone paint is based on the consumption of 1m 2 The sample is sprayed, the mass of the real stone paint used for spraying is recorded, and the mass of the fallen sand is collected at the bottom of the sample with plastic film. The sand falling rate = the mass of the fallen sand / the mass of the real stone paint used.
[0166] The reference standards and limits for the reflective thermal insulation real stone paint test items are shown in Table 12 below. The test results of the basic performance, reflective thermal insulation effect and lightweight effect of the reflective thermal insulation real stone paint in Examples 1-4 are shown in Table 13. The test results of the basic performance, reflective thermal insulation effect and lightweight effect of the reflective thermal insulation real stone paint in Comparative Examples 1-7 are shown in Table 14.
[0167] Table 12 Reference standards and limits for reflective heat-insulating real stone paint test items
[0168] Test items Test Method Evaluation Criteria Sunlight reflectance (low brightness) GB / T 25261-2018 ≥0.25 Near infrared reflectance (low brightness) GB / T 25261-2018 ≥0.40 Hemispherical emissivity (low brightness) GB / T 25261-2018 ≥0.85 Thermal conductivity / [W / (mK)] GB / T 25261-2018 ≤0.08 Surface drying time / h JG / T 24-2018 ≤4h Initial drying crack resistance JG / T 24-2018 3h no cracking Low temperature stability (3 cycles) JG / T 24-2018 No deterioration Thermal storage stability (15d) JG / T 24-2018 No caking, mildew, condensation or change in composition <![CDATA[Consumption of real stone paint / (kg / m 2 )]]> Refer to the above method Measured Construction JG / T 24-2018 Barrier-free application Water absorption / (2h / g) JG / T 24-2018 ≤2.0 Water resistance (96h) JG / T 24-2018 No abnormality Alkali resistance (96h) JG / T 24-2018 No abnormality Coating temperature change resistance (5 cycles) JG / T 24-2018 No abnormality Stain resistance / grade JG / T 24-2018 ≤2 Bond strength (standard state) / MPa JG / T 24-2018 ≥0.60 Bond strength (freeze-thaw cycle) / MPa JG / T 24-2018 ≥0.40
[0169] Table 13 Test results of basic properties, reflective heat insulation effect and lightweight effect of reflective heat insulation real stone paint in Examples 1-4
[0170] Test items Example 1 Example 2 Example 3 Example 4 Sunlight reflectance (low brightness) 0.40 0.41 0.36 0.48 Near infrared reflectance (low brightness) 0.55 0.56 0.51 0.60 Hemispherical emissivity (low brightness) 0.92 0.92 0.91 0.94 Thermal conductivity / [W / (m·K)] 0.035 0.042 0.050 0.028 Surface drying time / h 4h dry 4h dry 4h dry 4h dry Initial drying crack resistance 3h no cracking 3h no cracking 3h no cracking 3h no cracking Low temperature stability (3 cycles) No deterioration No deterioration No deterioration No deterioration Thermal storage stability (15d) No abnormality No abnormality No abnormality No abnormality <![CDATA[Consumption of real stone paint / (kg / m 2 )]]> 1.5 1.2 1.5 1.1 Sand loss rate / % 0.5 0.4 0.5 0.3 Construction No abnormality No abnormality No abnormality No abnormality Water absorption / (2h / g) 0.78 0.82 0.55 0.92 Water resistance (96h) No abnormality No abnormality No abnormality No abnormality Alkali resistance (96h) No abnormality No abnormality No abnormality No abnormality Coating temperature change resistance (5 cycles) No abnormality No abnormality No abnormality No abnormality Stain resistance / grade Level 1 Level 1 Level 1 Level 1 Bond strength (standard state) / MPa 0.92 1.12 0.85 1.23 Bond strength (freeze-thaw cycle) / MPa 0.88 0.95 0.63 1.02
[0171] Table 14 Test results of basic performance, reflective heat insulation effect and lightweight effect of reflective heat insulation real stone paint in comparative examples 1-7
[0172]
[0173]
[0174] Table 13 shows the basic performance, reflective heat insulation effect and lightweight effect test results of the reflective heat insulation real stone paint in Examples 1-4, and Table 14 shows the basic performance, reflective heat insulation effect and lightweight effect test results of the reflective heat insulation real stone paint in Comparative Examples 1-7. Combining the test results in Table 13 and Table 14, it can be seen that:
[0175] Compared with Comparative Example 1 (using ordinary silicone-acrylic emulsion) or Comparative Example 2 (using ordinary silicone-acrylic emulsion and hollow glass microspheres), the reflective heat-insulating real stone paint in Example 1 (using heat-insulating emulsion) has increased solar reflectance, near-infrared reflectance, and hemispherical emissivity, and significantly reduced thermal conductivity, indicating that the core-shell type heat-insulating emulsion can completely replace the hollow glass microspheres and provide better reflective heat-insulating effects. In addition, the storage stability of the reflective heat-insulating real stone paint with the addition of the core-shell type heat-insulating emulsion is improved.
[0176] Compared with Comparative Examples 4, 5, 6 and 7, the solar reflectance, near-infrared reflectance and hemispherical emissivity of the real stone paint in Example 1 are increased, and the thermal conductivity is significantly reduced, indicating that it has good reflective heat-insulating effect; while in Comparative Examples 4, 5 and 6, since only one or two of the core-shell type thermal insulation emulsion, reflective thermal insulation coated stone and reflective thermal insulation rock flakes are used as functional raw materials, the thermal insulation effect of the real stone paint is only slightly improved compared with that of Comparative Example 7, indicating that in the reflective thermal insulation real stone paint provided by the present invention, there is a synergistic effect between the functional raw materials core-shell type thermal insulation emulsion, reflective thermal insulation coated stone and reflective thermal insulation rock flakes, and the three need to be used at the same time to significantly improve the reflective heat-insulating effect of the real stone paint.
[0177] Compared with Example 2, Comparative Example 3 and Comparative Example 4, the stone powder, pigment powder and reflective insulating rock flakes used in Example 1 can enhance the hiding power of real stone paint, reduce the consumption of real stone paint, reduce the sand loss rate of real stone paint during construction, and achieve lightweight; and while achieving lightweight, the reflective insulation effect is not reduced.
[0178] The reflective heat-insulating real stone paint provided by the present invention replaces the hollow glass microspheres in the traditional functional filler with a core-shell type heat-insulating emulsion, thereby improving the reflective heat-insulating effect and storage stability of the real stone paint, and overcoming the defects of poor construction performance and difficulty in meeting the standards for medium and low brightness; the coordinated use of several functional raw materials such as the core-shell type heat-insulating emulsion, the reflective heat-insulating coated stone and the reflective heat-insulating rock flakes significantly improves the heat-insulating effect of the real stone paint; compared with the existing reflective heat-insulating real stone paint, the construction consumption is reduced by more than 50%, and while improving the reflective heat-insulating effect, it also achieves lightweight, which can meet the application requirements of heat-insulating materials in the field of energy-saving buildings.
Claims
1. A reflective heat-insulating real stone paint, characterized in that: The preparation raw materials include: base material, reflective heat-insulating coating stone, reflective heat-insulating rock flakes, stone powder and pigment powder; The raw materials for preparing the reflective heat-insulating coated stone include coating liquid and stone; the coating liquid includes heat-insulating emulsion, acrylic emulsion and film-forming aid; The raw materials for preparing the reflective heat-insulating rock sheet include heat-insulating emulsion, elastic pure acrylic emulsion and expanded pearlite powder; The raw materials for preparing the base material include heat insulation emulsion.
2. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The thermal insulation emulsion is a core-shell emulsion; Preferably, the particle size of the core-shell emulsion is 1000-2000 nm, and the core particle size is 300-600 nm; Preferably, the solid content of the core-shell emulsion is 40-55 wt %.
3. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The reflective heat-insulating real stone paint comprises the following raw materials by weight: 20-30 parts of base material, 60-80 parts of reflective heat-insulating coated stone, 0.1-2 parts of reflective heat-insulating rock flakes, 3-6 parts of stone powder, and 0.1-2 parts of pigment powder.
4. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The base material includes the following raw materials by weight: 40-60 parts of thermal insulation emulsion, 30-50 parts of water, 0.1-1 part of cellulose, 0.1-1 part of pH regulator, 0.1-3 parts of film-forming aid, 0.1-1 part of antifreeze agent, 0.1-1 part of defoaming agent, and 0.1-1 part of preservative.
5. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The reflective heat-insulating coated stone material comprises the following raw materials by weight: 5-15 parts of coating liquid material and 95-105 parts of stone material; the coating liquid material comprises the following raw materials by weight: 25-35 parts of heat-insulating emulsion, 55-65 parts of acrylic emulsion and 1-2 parts of film-forming aid; Preferably, the stone comprises expanded perlite.
6. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The reflective heat-insulating rock sheet comprises the following raw materials by weight: 35-45 parts of heat-insulating emulsion, 35-45 parts of elastic pure acrylic emulsion, and 15-25 parts of expanded pearlite powder; Preferably, the thickness of the reflective heat-insulating rock sheet is 0.01-0.1 mm; Preferably, the particle size of the reflective heat-insulating rock pieces is 0.3-1.5 mm.
7. The reflective heat-insulating real stone paint according to claim 1, characterized in that: The stone powder includes calcite powder; And / or, the particle size of the stone powder is 180-250 mesh; And / or, the particle size of the pigment powder is 200-300 mesh.
8. The reflective heat-insulating real stone paint according to claim 4, characterized in that: The cellulose includes hydrophobically modified hydroxyethyl cellulose ether.
9. The method for preparing the reflective heat-insulating real stone paint according to any one of claims 1 to 8, characterized in that: The following steps are involved: The prepared raw materials are mixed to obtain the reflective heat-insulating real stone paint.
10. Application of the reflective heat-insulating real stone paint according to any one of claims 1 to 8 in the field of energy-saving buildings.
Citation Information
Patent Citations
Durable self-cleaning core-shell acrylic emulsion for stone-like coatings, and preparation method thereof
CN110669161A
Inorganic reflective heat-insulation light ceramic colored stone coating and preparation method thereof
CN114525046A
Organosilicon modified acrylic emulsion, water-based heat insulation coating, water-based heat reflection finishing coat and preparation method thereof
CN118085194A
Real stone paint as well as preparation method and application thereof
CN118460019A