Graphene / spherical aluminum oxide / polyurethane laminated composite flexible heat-conducting interface material as well as preparation method and application thereof

Through the laminated structure of graphene/spherical alumina/polyurethane laminated composite, the problem that traditional thermal interface materials cannot meet the thermal management needs of high power density electronic products is solved, and high-performance thermal conductivity and insulation performance are achieved, suitable for electronics Devices and smart wearable fields.

CN119039865AActive Publication Date: 2024-11-29ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202410957480.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-29
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Traditional thermal interface materials cannot meet the efficient thermal management needs of high-power density electronics and wearable electronics, and excessive filler filling will lead to agglomeration and affect heat transfer.

Method used

Using graphene/spherical alumina/polyurethane laminated composite materials, a unique laminated structure is constructed by alternately coating graphene and spherical alumina layers, adjusting the stacking order of graphene and alumina to improve thermal conductivity, and through different Size spherical alumina filled and graphene flakes surrounded by reduced interface thermal resistance.

Benefits of technology

Achieve high-performance thermal interface material, with an in-plane thermal conductivity of 15.433W/mK and an out-plane thermal conductivity of 22.433W/mK. It has excellent flexibility, mechanical properties and insulation properties, and is suitable for high-power electronic devices and intelligent wearables. field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039865A_ABST
    Figure CN119039865A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of heat-conducting interface materials, in particular to a graphene / spherical aluminum oxide / polyurethane laminated composite flexible heat-conducting interface material and a preparation method thereof. A polyurethane matrix is filled with spherical aluminum oxide of different sizes, and the high-performance graphene / spherical aluminum oxide / polyurethane laminated composite flexible heat-conducting interface material (the highest in-plane heat conductivity coefficient can reach 15.433 W / mK, and the highest out-plane heat conductivity coefficient can reach 22.433 W / mK) is obtained by changing the stacking sequence of graphene and aluminum oxide. The graphene / spherical aluminum oxide / polyurethane laminated composite flexible heat-conducting interface material prepared by the invention is stable in structure, has excellent flexibility, mechanical property and certain insulating property, and has wide application scenarios in the fields of electronic devices and intelligent wearing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal conductive interface materials, and in particular to a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, a preparation method and application thereof. Background Art

[0002] Nowadays, electronic devices have become an indispensable part of our daily life. With the increasing miniaturization, integration and multi-function of electronic devices, the power density and heat output per unit volume have increased significantly. If the heat cannot be effectively dissipated, it will have an adverse effect on its performance and service life. Overheating of microelectronic devices has become a bottleneck restricting the development and application of high-frequency and high-power devices and systems in advanced communication information technology.

[0003] At present, the rapid deployment of 5G technology in the field of consumer electronics has put forward higher requirements and new challenges for more efficient thermal management. The thermal conductivity and other properties of traditional thermal conductive interface materials can no longer meet the growing demand for high-power density electronic products and wearable electronic products.

[0004] Traditional thermal conductive interface materials prepared by filling thermal conductive fillers often have filler agglomeration inside due to the addition of excessive thermal conductive fillers, which affects the effective transfer of heat. The high-performance thermal conductive interface materials currently required require thermal conductive fillers to form a stable, uniform and effective thermal conductive path in the polymer matrix. On the premise of having high thermal conductivity, they also have excellent insulation and mechanical properties, and have a long service life, low production cost and conditions for large-scale production and preparation. They are currently an important direction for the development of thermal conductive composite materials. Summary of the invention

[0005] The present invention is made to solve the above-mentioned problems, and its purpose is to provide a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, its preparation method and application, so as to solve the above-mentioned technical problems.

[0006] The first aspect of the present invention provides a method for preparing a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, characterized in that it comprises the following steps:

[0007] S1. Preparation of graphene / polyurethane slurry: mixing water-based polyurethane, water-based polymer dispersant and cross-linking agent and adding graphene powder to obtain a first mixed solution, adjusting the viscosity and preliminarily stirring to obtain graphene / polyurethane slurry after vacuum degassing and stirring;

[0008] S2. Preparation of spherical alumina / polyurethane slurry: Spherical alumina powder and a dispersant are mixed and ultrasonically treated, and then water-based polyurethane and a cross-linking agent are added to obtain a second mixed solution, which is mixed and stirred evenly, and then subjected to vacuum degassing and stirring treatment to obtain a spherical alumina / polyurethane slurry;

[0009] S3. Preparation of graphene / spherical alumina / polyurethane laminated composite film: using polymethyl methacrylate as a substrate, alternately applying the graphene / polyurethane slurry in S1 or the spherical alumina / polyurethane slurry prepared in S2 on the polymethyl methacrylate substrate to obtain a graphene / polyurethane slurry layer or a spherical alumina / polyurethane slurry layer, drying each layer after coating before coating the next layer, and after alternately coating several layers, using the graphene / polyurethane slurry layer or the spherical alumina / polyurethane slurry layer as the outermost layer and drying it to obtain a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material after drying.

[0010] The present invention fills a polyurethane matrix with spherical alumina, which is surrounded by graphene sheets to form a unique laminated composite structure film. By changing the stacking order of graphene and alumina, controllable adjustment is performed to obtain a high-performance graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material (the in-plane thermal conductivity can reach up to 15.433 W / mK, and the out-of-plane thermal conductivity can reach up to 22.433 W / mK).

[0011] The graphene / spherical aluminum oxide / polyurethane laminated composite flexible thermal conductive interface material prepared by the invention has a stable structure, excellent flexibility, mechanical properties and certain insulation properties.

[0012] The present invention adopts alternating continuous coating technology, which is simple and controllable, low-cost, and easy to mass produce. It has a wide range of application scenarios in the field of electronic devices and smart wearables.

[0013] In some embodiments of the present invention, the mass of the graphene powder added in S1 is 8-15% of the mass of the first mixed solution.

[0014] In the present invention, by controlling the mass ratio of graphene powder, the prepared graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material has good mechanical properties and insulation properties.

[0015] In some embodiments of the present invention, the mass of the graphene powder added in S1 is 12-15% of the mass of the first mixed solution.

[0016] In some embodiments of the present invention, in S1, the cross-linking agent is aziridine, and the added amount of the aqueous polymer dispersant and aziridine is 1-5% of the mass of the first mixed liquid respectively; the viscosity is adjusted by adding water and ethanol, and the added amount of water and ethanol is 1-9% of the mass of the first mixed liquid in total; the initial stirring time is 10-60 minutes; and the vacuum degassing stirring time is 5-15 minutes.

[0017] In some embodiments of the present invention, the mass of the spherical aluminum oxide added to S2 is 50-60% of the mass of the second mixed liquid.

[0018] The present invention reduces the fracture strength of the composite material by adding aluminum oxide, thereby significantly improving the insulation performance and out-of-plane thermal conductivity of the composite material.

[0019] When the mass of graphene powder added to S1 is 12-15% of the mass of the first mixed liquid and the mass of spherical alumina added to S2 is 50-60% of the mass of the second mixed liquid, graphene and alumina can form a good synergistic effect, greatly improving the thermal conductivity inside and outside the composite material surface, and having good mechanical properties and insulation properties.

[0020] In some embodiments of the present invention, in S2, the particle sizes of the spherical alumina include 5 μm, 10 μm, 45 μm, and 70 μm, and the addition ratio of the spherical alumina with particle sizes of 5 μm, 10 μm, 45 μm, and 70 μm is 1:1~2:1~2:1~3.

[0021] The present invention fills a polyurethane matrix with spherical alumina of different sizes, which is surrounded by graphene sheets to form a unique laminated composite structure film; the large-particle spherical alumina can make the two-dimensional graphene sheets adhere, significantly improve the orientation of graphene in the vertical direction, and reduce the interface thermal resistance between graphene, alumina and the polyurethane matrix.

[0022] In some embodiments of the present invention, in S2, the dispersant is a mixed dispersion of acetone and nano-alumina ethanol, and the amount of the dispersant added is 3 to 10% of the mass of the second mixed liquid; the cross-linking agent is aziridine, and the amount of aziridine added is 1 to 5% of the mass of the water-based polyurethane, the ultrasonic time is 30 to 100 minutes, the mixing and stirring time is 10 to 60 minutes, and the vacuum degassing and stirring time is 5 to 15 minutes.

[0023] In some embodiments of the present invention, in S3, the coating thickness of the graphene / polyurethane slurry layer is 10 to 40 μm, the coating thickness of the spherical alumina / polyurethane slurry is set to 70 to 90 μm, the number of coating layers is 3 to 11 layers, and the total coating thickness is 90 to 740 μm.

[0024] The present invention can adjust the thickness of the film by changing the number of coated layers and the coating thickness, thereby obtaining a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material with different properties, which can be arbitrarily cut according to actual needs and has a wide range of applications.

[0025] The second aspect of the present invention provides a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, wherein the graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material is prepared according to any preparation method described in the first aspect.

[0026] The third aspect of the present invention provides an application of the graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material as described in the second aspect, and the graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material is used in the field of high-power electronic devices.

[0027] By implementing the above technical solution, the present invention has the following beneficial effects:

[0028] 1. The present invention fills a polyurethane matrix with spherical alumina of different sizes, which is surrounded by graphene sheets to form a unique laminated composite structure film; large-particle spherical alumina can make two-dimensional graphene sheets adhere, significantly improve the orientation of graphene in the vertical direction, and reduce the interfacial thermal resistance between graphene, alumina and polyurethane matrix, thereby obtaining a high-performance graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material (the in-plane thermal conductivity can reach 15.433W / mK, and the out-of-plane thermal conductivity can reach 22.437W / mK).

[0029] 2. The graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material prepared by the present invention has a stable structure, excellent flexibility, mechanical properties and certain insulation properties; the thickness of the film can be adjusted by changing the number of coated layers, and can be arbitrarily cut according to actual needs, and has a wide range of applications.

[0030] 3. The present invention adopts alternating continuous coating technology, which is simple and controllable, low-cost and easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of the structure of the graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material provided by the present invention;

[0032] Figure 2 The present invention is a flow chart of the preparation method of graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material. DETAILED DESCRIPTION

[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is described in detail below in conjunction with embodiments and drawings.

[0034] Example 1

[0035] S1, preparation of graphene / polyurethane slurry: weigh 17g of waterborne polyurethane, add 0.3g of waterborne polymer dispersant and 0.3g of aziridine crosslinking agent, mix, weigh 0.6g of graphene powder, slowly add while stirring, initially stir for 30min, add 1.8g of ethanol at the same time, adjust the viscosity, and obtain a first mixed solution when the solution viscosity is appropriate, then vacuum degassing and stirring for 10min, and configure it into graphene / polyurethane slurry for standby use;

[0036] S2. Preparation of spherical alumina / polyurethane slurry: weigh 24 g of 70 μm, 45 μm, 10 μm, and 5 μm spherical alumina mixed powder (3:2:2:1), add 3.6 g of acetone and nano-alumina ethanol dispersion (1:2), mix and ultrasonically treat for 30 minutes, then add 20 g of waterborne polyurethane and 0.4 g of aziridine crosslinking agent, mix and stir for 30 minutes, finally degas and stir in vacuum for 10 minutes to prepare spherical alumina / polyurethane slurry for use;

[0037] S3, preparation of graphene / spherical alumina / polyurethane laminated composite film: Use a battery coating machine to alternately coat the slurry prepared in the previous step on the PMMA substrate by first coating the graphene / polyurethane slurry to prepare the graphene layer and then coating the spherical alumina / polyurethane slurry to prepare the alumina layer. Each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternating coating 3 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0038] Example 2

[0039] The preparation process is similar to that of Example 1, except that in step S3 of Example 2, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After coating 3 layers alternately, fully dry at room temperature for 12 hours; cut neatly, and the preparation is completed.

[0040] Example 3

[0041] The preparation process is similar to that of Example 1, except that in step S3 of Example 3, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating the graphene layer and then coating the alumina layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After coating 11 layers alternately, fully dry at room temperature for 12 hours; cut neatly, and the preparation is completed.

[0042] Example 4

[0043] The preparation process is similar to that of Example 3, except that in step S3 of Example 4, the prepared slurry is alternately coated on the PMMA substrate using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer. Each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternately coating 11 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0044] Example 5

[0045] The preparation process is similar to that of Example 1, except that the ratio of graphene / polyurethane slurry preparation is changed in step S1 of Example 5. The specific operation of S1 is as follows:

[0046] S1. Weigh 17g of waterborne polyurethane, add 0.3g of waterborne polymer dispersant and 0.3g of aziridine crosslinking agent, mix, then weigh 1.6g of graphene powder, slowly add while stirring, initially stir for 30min, and at the same time add 0.2g of ethanol and 0.6g of deionized water, adjust the viscosity, and when the solution viscosity is suitable, obtain the first mixed solution, then stir for 10min through vacuum degassing, and configure it into graphene / polyurethane slurry for standby use.

[0047] The remaining steps are consistent with those in Example 1.

[0048] Example 6

[0049] The preparation process is similar to that of Example 5, except that in step S3 of Example 6, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After three layers are alternately coated, they are fully dried at room temperature for 12 hours; and the preparation is completed by neatly cutting.

[0050] Example 7

[0051] The preparation process is similar to that of Example 5, except that in step S3 of Example 7, the prepared slurry is alternately coated on the PMMA substrate using a battery coating machine in the order of first coating the graphene layer and then coating the aluminum oxide layer. Each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternately coating 11 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0052] Example 8

[0053] The preparation process is similar to that of Example 6, except that in step S3 of Example 8, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After coating 11 layers alternately, fully dry at room temperature for 12 hours; cut neatly, and the preparation is completed.

[0054] Example 9

[0055] The preparation process is similar to that of Example 1, except that the ratio of graphene / polyurethane slurry preparation is changed in step S1 of Example 9. The specific operation of S1 is as follows:

[0056] S1. Weigh 16g of waterborne polyurethane, add 0.3g of waterborne polymer dispersant and 0.3g of aziridine crosslinking agent, mix, then weigh 2.4g of graphene powder, slowly add while stirring, initially stir for 30min, and at the same time add 1g of deionized water to adjust the viscosity. When the viscosity of the solution is suitable, a first mixed solution is obtained, and then vacuum degassing and stirring for 10min are performed to prepare a graphene / polyurethane slurry for standby use.

[0057] The remaining steps are consistent with those in Example 1.

[0058] Example 10

[0059] The preparation process is similar to that of Example 9, except that in step S3 of Example 10, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After three layers are alternately coated, they are fully dried at room temperature for 12 hours; and the preparation is completed by neatly cutting.

[0060] Embodiment 11

[0061] The preparation process is similar to that of Example 9, except that, in step S3 of Example 11, the prepared slurry is alternately coated on the PMMA substrate using a battery coating machine in the order of first coating the graphene layer and then coating the alumina layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternately coating 11 layers, fully dry at room temperature for 12 hours; cut neatly, and the preparation is completed.

[0062] Example 12

[0063] The preparation process is similar to that of Example 10, except that, in step S3 of Example 12, the prepared slurry is alternately coated on the PMMA substrate using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternately coating 11 layers, fully dry at room temperature for 12 hours; cut neatly, and the preparation is completed.

[0064] Example 13

[0065] The preparation process is similar to that of Example 1, except that in step S1 of Example 13, the ratio of graphene / polyurethane slurry preparation is changed. The specific operation of S1 is as follows:

[0066] S1. Weigh 15g of waterborne polyurethane, add 0.3g of waterborne polymer dispersant and 0.3g of aziridine crosslinking agent, mix, then weigh 3g of graphene powder, slowly add while stirring, initially stir for 30min, and at the same time add 1.4g of deionized water to adjust the viscosity. When the viscosity of the solution is suitable, a first mixed solution is obtained, and then vacuum degassing and stirring for 10min are performed to prepare a graphene / polyurethane slurry for standby use.

[0067] The remaining steps are consistent with those in Example 1.

[0068] Embodiment 14

[0069] The preparation process is similar to that of Example 13, except that in step S3 of Example 14, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After coating 3 layers alternately, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0070] Embodiment 15

[0071] The preparation process is similar to that of Example 1, except that in step S1 of Example 15, the ratio of graphene / polyurethane slurry preparation is changed. The specific operation of S1 is as follows:

[0072] S1, weigh 16g of waterborne polyurethane, add 0.3g of waterborne polymer dispersant, 0.3g of aziridine crosslinking agent, mix, weigh 2.4g of graphene powder, slowly add while stirring, initially stir for 30min, add 1g of deionized water at the same time, adjust the viscosity, wait until the solution viscosity is suitable, obtain the first mixed solution, then stir for 10min through vacuum degassing, and configure into graphene / polyurethane slurry for standby;

[0073] The difference is that in step S2 of Example 15, the amount of the spherical alumina mixed powder added is changed, and the specific operation of S2 is as follows:

[0074] S2. Preparation of spherical alumina / polyurethane slurry: Weigh 36 g of 70 μm, 45 μm, 10 μm, and 5 μm spherical alumina mixed powder (3:2:2:1), add 3.6 g of acetone and nano-alumina ethanol dispersion (1:2), mix and ultrasonically treat for 30 minutes, then add 20 g of water-based polyurethane and 0.4 g of aziridine cross-linking agent, mix and stir for 30 minutes, finally degas and stir in vacuum for 10 minutes to prepare spherical alumina / polyurethane slurry for use.

[0075] The remaining steps are consistent with those in Example 1.

[0076] Example 16

[0077] The preparation process is similar to that of Example 15, except that in step S3 of Example 16, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After three layers are alternately coated, they are fully dried at room temperature for 12 hours; and the preparation is completed by neatly cutting.

[0078] Embodiment 17

[0079] The preparation process is similar to that of Example 15, except that in step S3 of Example 17, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating the graphene layer and then coating the aluminum oxide layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After coating 11 layers alternately, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0080] Embodiment 18

[0081] The preparation process is similar to that of Example 16, except that in step S3 of Example 18, the prepared slurry is alternately coated on the PMMA substrate using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer. Each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternately coating 11 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0082] Embodiment 19

[0083] The preparation process is similar to that of Example 15, except that in step S3 of Example 19, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating the graphene layer and then coating the alumina layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternating coating of 5 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0084] Embodiment 20

[0085] The preparation process is similar to that of Example 16, except that in step S3 of Example 20, the prepared slurry is coated on the PMMA substrate by using a battery coating machine in the order of first coating an aluminum oxide layer and then coating a graphene layer, and each layer after coating is dried in an oven at 50°C for 2 minutes, and then coating is continued on the basis of the layer. After alternating coating of 5 layers, fully dry at room temperature for 12 hours; cut neatly to complete the preparation.

[0086] Comparative Example 1

[0087] The same as Example 15, except that the prepared graphene / polyurethane slurry and spherical alumina / polyurethane slurry are first blended and then 5 layers of coating are performed.

[0088] Comparative Example 2

[0089] The same as Example 15, except that only 5 layers of coating of spherical alumina / polyurethane slurry were prepared.

[0090] Comparative Example 3

[0091] The same as Example 15, except that only 5 layers of coating of graphene / polyurethane slurry were performed.

[0092] Performance Testing

[0093] The thermal interface materials obtained in Examples 1 to 20 and Comparative Examples 1 to 3 were subjected to performance tests, including thermal conductivity test using the German NETZSCH laser thermal conductivity tester LFA-467, the test method was carried out in accordance with the ASTM E1461 standard, and the thermal conductivity of the material was tested by using a circular sample with a diameter of 5.4 mm for three times and taking the average value; the breakdown voltage was tested using an electrical strength tester, the test was carried out using the ASTM D149 standard, and a circular sample with a diameter of 25 mm. 8 to 10 test points were measured and the average value was taken; the test results are shown in Table 1.

[0094] Table 1 Performance test results of thermal interface materials

[0095]

[0096] As can be seen from Table 1, the number of layers and thickness of the composite material can be adjusted according to the actual application field to obtain thermally conductive materials with different in-plane or out-of-plane thermal conductivity and insulation properties. It can be seen from the above embodiments that with the increase of graphene content, the in-plane thermal conductivity of the composite material is significantly improved; but the addition of graphene will reduce the insulation effect of the material. When the amount of graphene added increases to 15%, all properties are greatly reduced. The reason is that the content is too high, resulting in uneven coating and the existence of graphene agglomeration. The addition of aluminum oxide will weaken the fracture strength of the composite material and can significantly improve the insulation performance and out-of-plane thermal conductivity of the composite material. By comparing Comparative Examples 1, 2, and 3 with Examples 15 to 20, it can be concluded that at this ratio, graphene and aluminum oxide form a good synergistic effect, greatly improve the thermal conductivity inside and outside the plane, and have good mechanical properties and insulation properties.

[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, characterized in that: The following steps are involved: S1. Preparation of graphene / polyurethane slurry: mixing waterborne polyurethane, waterborne polymer dispersant and crosslinking agent and adding graphene powder to obtain a first mixed solution, adjusting the viscosity and preliminarily stirring to obtain graphene / polyurethane slurry after vacuum degassing and stirring; S2. Preparation of spherical alumina / polyurethane slurry: Spherical alumina powder and a dispersant are mixed and ultrasonically treated, and then water-based polyurethane and a cross-linking agent are added to obtain a second mixed solution, which is mixed and stirred evenly, and then subjected to vacuum degassing and stirring treatment to obtain a spherical alumina / polyurethane slurry; S3. Preparation of graphene / spherical alumina / polyurethane laminated composite film: using polymethyl methacrylate as a substrate, alternately applying the graphene / polyurethane slurry in S1 or the spherical alumina / polyurethane slurry prepared in S2 on the polymethyl methacrylate substrate to obtain a graphene layer or a spherical alumina layer, drying each layer after coating before coating the next layer, and after alternately coating several layers, using the graphene layer or the spherical alumina layer as the outermost layer and drying it, to obtain a graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material after drying.

2. The preparation method according to claim 1, characterized in that: The mass of the graphene powder added in S1 is 8-15% of the mass of the first mixed solution.

3. The preparation method according to claim 2, characterized in that: The mass of the graphene powder added in S1 is 12-15% of the mass of the first mixed solution.

4. The preparation method according to claim 3, characterized in that: In S1, the cross-linking agent is aziridine, and the added amounts of the aqueous polymer dispersant and aziridine are 1 to 5% of the mass of the first mixed liquid respectively; the viscosity is adjusted by adding water and ethanol, and the added amounts of water and ethanol are 1 to 9% of the mass of the first mixed liquid in total; the initial stirring time is 10 to 60 minutes; and the vacuum degassing stirring time is 5 to 15 minutes.

5. The preparation method according to claim 1, characterized in that: The mass of the spherical aluminum oxide added to S2 is 50-60% of the mass of the second mixed liquid.

6. The preparation method according to claim 5, characterized in that: In S2, the particle sizes of the spherical alumina include 5 μm, 10 μm, 45 μm, and 70 μm, and the addition ratio of the spherical alumina with particle sizes of 5 μm, 10 μm, 45 μm, and 70 μm is 1:1 to 2:1 to 2:1 to 3.

7. The preparation method according to claim 6, characterized in that: In S2, the dispersant is a mixed dispersion of acetone and nano-alumina ethanol, and the added amount of the dispersant is 3-10% of the mass of the second mixed liquid; the cross-linking agent is aziridine, and the added amount of aziridine is 1-5% of the mass of the water-based polyurethane, the ultrasonic time is 30-100 minutes, the mixing and stirring time is 10-60 minutes, and the vacuum degassing and stirring time is 5-15 minutes.

8. The method according to claim 1, characterized in that In S3, the coating thickness of the graphene / polyurethane slurry layer is 10-40 μm, the coating thickness of the spherical alumina / polyurethane slurry is set to 70-90 μm, the number of coating layers is 3-11 layers, and the total coating thickness is 90-740 μm.

9. A graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material, characterized in that: The graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material is prepared according to the preparation method according to any one of claims 1 to 8.

10. An application of the graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material as claimed in claim 9, characterized in that: The graphene / spherical alumina / polyurethane laminated composite flexible thermal conductive interface material is used in the field of high-power electronic devices.

Citation Information

Patent Citations

  • Graphite laminated composite material and preparation method thereof

    CN114771040A

  • Heat radiation sheet and method for manufacturing same

    KR1020150002191A

  • Heat discharging sheet and method for manufacturing the same

    US20160053155A1

  • Preparation method for graphite-oriented thermal interface material

    WO2022120700A1

Cited By

  • Graphene aluminum vapor chamber and preparation method thereof

    CN119653739A

  • High-thermal-conductivity graphene composite film and preparation method thereof

    CN121318455A