Methyl phenyl silicone resin for high-temperature-resistant petroleum pipeline finish paint and preparation method of methyl phenyl silicone resin

By optimizing raw materials and synthesis conditions, a high-performance methylphenyl silicone resin was developed, which solved the problem of insufficient performance of existing high-temperature resistant coatings in high temperature and high pollution environments, and achieved high-temperature decomposition without smoke and bonding strength High, anti-fouling and long-lasting properties, suitable for high-temperature resistant oil pipeline topcoat.

CN119039877APending Publication Date: 2024-11-29JIANGSU SANMU GRP CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411127207.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-temperature resistant silicone coatings are difficult to meet the impact resistance, high strength and wear resistance requirements of metal materials in high temperature and high pollution corrosion environments. The hydrogen chloride gas generated in the synthesis method causes the reaction system to be easily gelled, affecting the product. Low hazard and finished product performance.

Method used

By optimizing the raw materials and synthesis conditions, a methylphenyl silicone resin composed of methyl trichlorosilane, toluene, propylene glycol methyl ether acetate was developed, and the reaction conditions and component ratio were synthesized by hydrolysis and condensation method to control the reaction conditions and component ratios to ensure that The resin has high-temperature resistant petroleum pipeline topcoat with high temperature decomposition without smoke, high bonding strength, long-lasting stain resistance, high weather resistance and gloss.

Benefits of technology

It achieves high performance performance of resin at high temperatures, including high temperature decomposition without smoke, high bonding strength, long-lasting anti-fouling, high chemical resistance, high adhesion and good impact performance, and reduces production costs and hazards, suitable for high temperatures Petroleum pipe topcoat.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996781520000041
    Figure BDA0004996781520000041
  • Figure BDA0004996781520000051
    Figure BDA0004996781520000051
  • Figure BDA0004996781520000052
    Figure BDA0004996781520000052
Patent Text Reader

Abstract

The invention discloses methyl phenyl silicone resin for high-temperature-resistant petroleum pipeline finish paint and a preparation method of the methyl phenyl silicone resin. The methyl phenyl silicone resin is prepared from the following raw materials: methyl trichlorosilane, dimethyl dichlorosilane, phenyl trichlorosilane, diphenyl dichlorosilane, methylbenzene, dimethylbenzene, acetone, propylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, n-butyl alcohol, ionized water, tap water and the like. The methyl phenyl silicone resin is prepared by screening through a large number of experiments, adopting a hydrolysis method and a condensation method, and preferably adjusting an optimal methyl proportion and selecting a proper solvent system. The methyl phenyl silicone resin prepared by the invention has the advantages of simple and cheap raw materials, no smoking in high-temperature decomposition, high bonding strength, high activity, lasting antifouling property, high temperature resistance, high chemical resistance, high adhesive force, high glossiness and good impact property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat, which belongs to a polymer resin with wide application and excellent performance. It is a composite polymer compound formed by cross-linking polymerization of multiple methylphenylsilane monomers. The methylphenyl silicone resin has the advantages of excellent temperature resistance, chemical corrosion resistance, mechanical strength and the like. Background Art

[0002] The introduction of Si-O bonds in methylphenyl silicone resin gives it obvious advantages in mechanical properties, thermal elasticity, adhesion, gloss, and compatibility with organic and inorganic fillers. It can be used as high-temperature resistant insulating varnish, high-temperature resistant adhesive, high-temperature resistant molding packaging material, high-temperature resistant coating, ablative material, silicone resin micropowder and other products. It is the largest and most widely used variety of silicone resin at present.

[0003] With the advent of the 21st century, the rapid development of modern industry and military and other industries, people have higher and higher requirements for the performance of metal materials. Not only do they need to operate at higher temperatures and more harsh high-pollution corrosive environments, but they also need to have various properties such as impact resistance, high-strength mechanical properties and wear resistance. Ordinary organic coatings can hardly protect metal materials. The development of high-temperature resistant organic coatings with better performance is becoming more and more urgent, among which the development of high-temperature resistant organosilicon coatings is more prominent. As a film-forming material of coatings, organosilicon resin is a key factor in the performance of coatings. Its unique thermal stability and oxidation stability make silicone resin widely used in coatings. There are many methods for synthesizing organosilicon resins. Among them, the method of synthesizing methylphenyl silicone resin by hydrolysis and condensation using organochlorosilane as raw material has attracted attention. The raw materials of this method are produced by the direct method, the raw materials are easy to obtain, the output is large, and the cost is low. However, a large amount of hydrogen chloride gas is generated during the reaction of this method. When hydrogen chloride gas dissolves in water, it releases heat. The generated hydrochloric acid and heat accelerate the spontaneous condensation reaction of silanol, an intermediate of the hydrolysis reaction, making the reaction system easy to gel.

[0004] The invention develops a methyl phenyl silicone resin for high-temperature-resistant petroleum pipeline topcoat by a large number of experimental screenings, optimization of different raw materials and selection of synthesis conditions. The raw materials are simple, cheap and the finished product has low hazard. The methyl bond of chlorosilane has the characteristics of high activity and being more conducive to electrophilic substitution reaction. The phenyl bond of chlorosilane has the advantages of low volatility, good film-forming property and weather resistance. The methyl phenyl silicone resin has the advantages of no smoke when decomposed at high temperature, high bonding strength, weather resistance, long-lasting antifouling, high temperature resistance, high chemical resistance, high adhesion, high gloss and good impact performance. Summary of the invention

[0005] Purpose of the invention: The invention is to preferably obtain a methylphenyl silicone resin for high-temperature resistant petroleum pipeline topcoat which has high application performance, high temperature decomposition without smoke, high activity, long-lasting antifouling, high temperature resistance, high chemical resistance, high adhesion, high gloss and good impact performance. Another purpose of the invention is to provide a method for preparing the resin.

[0006] Technical solution, in order to achieve the above purpose, the technical solution adopted by the present invention is:

[0007] A methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat is made from the following raw materials:

[0008] Component A: one of monomethyltrichlorosilane, dimethyldichlorosilane, monophenyltrichlorosilane, diphenyldichlorosilane or a combination thereof;

[0009] Component B: one of toluene, xylene, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, or a combination thereof;

[0010] Component C: one or a combination of toluene, xylene, acetone, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, n-butanol, ionized water, and tap water;

[0011] Component D: one of zinc octoate, calcium octoate, isopropyl titanate or a combination thereof.

[0012] As a preferred embodiment, the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat described above is made of the following raw materials in weight percentage:

[0013] Component A 12-20%, component B 15-35%, component C 50-70%, D 0-1%.

[0014] As a preferred embodiment, the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat described above is made of the following raw materials in weight percentage:

[0015] Component A: 16.2%; Component B: 21.6%; Component C: 61.7% and Component D: 0.5%.

[0016] As a preferred embodiment, the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat described above is made of the following raw materials by weight: 124.5g of monomethyltrichlorosilane, 226.7g of dimethyldichlorosilane, 385.5g of monophenyltrichlorosilane, 73.3g of diphenyldichlorosilane, 1080g of propylene glycol methyl ether acetate, 510g of propylene glycol methyl ether acetate, 2600g of ionized water, and 2.8g of zinc isooctanoate.

[0017] As a preferred embodiment, the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat described above is made of the following raw materials by weight: 150.3g of monomethyltrichlorosilane, 196.2g of dimethyldichlorosilane, 443.5g of monophenyltrichlorosilane, 760g of xylene, 350g of xylene, 3100g of ionized water, and 2.9g of zinc isooctanoate.

[0018] The preparation method of the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat of the present invention comprises the following steps:

[0019] (1) First, add a certain amount of component A and component B into a reaction container, stir evenly to form a mixture A, and transfer the mixture A into a constant pressure dropping funnel for standby use;

[0020] (2) Add component C into the reaction vessel, start stirring, heat the mixture to 20-30° C. in a water bath, and slowly add the mixture A in step (1) dropwise; continue the addition for 4-6 hours;

[0021] (3) When the addition is completed, continue to maintain the temperature at 25-33°C for a period of time. When the maintenance is completed, let it stand, then separate the lower layer of acid water, wash the upper layer of solvent silicon with tap water, the pH test paper is neutral, and the acid value is 0-1 mgKOH / g;

[0022] (4) After the solvent silicon in step (3) is vacuum desolventized, component D is added and the temperature is raised to carry out a reflux condensation reaction. When the viscosity of the resin increases significantly and becomes viscous, it is cooled and a certain amount of component B is added to obtain methylphenyl silicone resin.

[0023] The method for preparing the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat of the present invention comprises the following steps:

[0024] (1) First, add a certain amount of component A and component B into a 3000 ml four-necked flask and stir to obtain a mixture A. Transfer the mixture A into a constant pressure dropping funnel and set aside;

[0025] (2) Add component C to a 5000 ml four-necked flask, start stirring, heat to 20° C. in a water bath, and slowly add mixture A dropwise at a rate of 1 drop / 1 second; maintain the temperature in the four-necked flask between 20-38° C. When the temperature exceeds 35° C., stop heating in the water bath, add ice cubes to cool down and maintain the process temperature at 23-33° C., and continue adding dropwise for 4-6 hours;

[0026] (3) When the step (2) is completed, the temperature is maintained at 25-33° C. for half an hour. After the maintenance is completed, the mixture is allowed to stand for half an hour. The lower layer of acid water is then separated and the upper layer of solvent silicon is washed 6 times with tap water until the pH test paper is neutral and the acid value is 0-1 mgKOH / g.

[0027] (4) After the solvent silicon in step (3) is vacuum desolventized, component D is added, the temperature is raised, and reflux condensation reaction is carried out. When the temperature is maintained at 158° C. and the viscosity of the resin increases significantly and becomes viscous, the resin is cooled and a certain amount of component B is added to obtain methylphenyl silicone resin.

[0028] As a preferred embodiment, in the method for preparing the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat described above, after the materials in step (1) are stirred evenly, they are transferred to a constant pressure funnel and then nitrogen is passed throughout the process to prevent premature reaction with water vapor in the air and monomer leakage to pollute the environment;

[0029] When the temperature in the four-necked flask in step (2) reaches 25°C, slowly add mixture A dropwise and observe whether there is any leakage to prevent the material from running, bubbling or leaking;

[0030] When the temperature in the four-necked flask of step (3) is maintained at 25-33°C for 4-6 hours, the process temperature is well controlled. In the middle and late stages of the dropwise addition, the reaction is more intense and the temperature rises rapidly. Ice needs to be added in advance to control the temperature to be 3°C lower than the maximum process temperature.

[0031] After the reaction in step (4) is completed, the lower layer of acid water must be completely removed during each water washing. Finally, the pH test paper is neutral, and the acid value measured by acid-base titration method is 0-1 mgKOH / g;

[0032] When step (5) starts, pay attention to temperature increase to prevent material rushing (the boiling point of the water-solvent mixture is uncertain); in the late stage of the reaction, the material reacts violently, so always observe the situation to prevent the material from rising too fast and spraying. After the condensation reaction is completed, add component B when it is cooled to 130°C, and control the solid content, viscosity, acid value, etc. After the control is qualified, cool it to below 80°C and discharge the material to obtain the product.

[0033] Beneficial effects: The present invention has the following advantages:

[0034] The present invention adopts a hydrolysis method and a condensation method through a large number of experimental screenings, and at the same time preferably adjusts the optimal methyl ratio and selects a suitable solvent system of methyl phenyl silicone resin. The methyl phenyl silicone resin for high temperature resistant petroleum pipeline topcoat of the present invention has comprehensive properties such as no smoke during high temperature decomposition, high bonding strength, high activity, long-lasting antifouling, high temperature resistance, high adhesion, high hardness, good impact, etc., and has relatively low viscosity, relatively reasonable cost, and strong practicality. DETAILED DESCRIPTION

[0035] Example 1

[0036] 1. A method for preparing a methylphenyl silicone resin for a high temperature resistant petroleum pipeline topcoat, comprising the following steps:

[0037] (1) First, 124.5 g of monomethyltrichlorosilane, 226.7 g of dimethyldichlorosilane, 385.5 g of monophenyltrichlorosilane, 73.3 g of diphenyldichlorosilane, and 1080 g of propylene glycol methyl ether acetate were added to a 3000 ml four-necked flask, and nitrogen was passed through the flask for protection. The mixture was stirred to obtain a mixture A, and the mixture A was transferred to a constant pressure dropping funnel for standby use;

[0038] (2) Add 510 g of propylene glycol methyl ether acetate and 2600 g of ionized water into a 5000 ml four-necked flask, start stirring, heat the mixture to 23° C. with a water bath, and slowly add the mixture A of step (1) dropwise at a rate of 1 drop / 1 second; maintain the temperature in the four-necked flask between 23 and 33° C. When the temperature exceeds 29° C., stop heating in the water bath, add ice cubes to cool the mixture to maintain the process temperature at 23-33° C., and continue adding dropwise for 5 hours;

[0039] (3) When the addition is completed, continue to maintain the temperature at 25-33°C for half an hour. After the maintenance is completed, let it stand for half an hour, then separate the lower layer of acid water, and wash the upper layer of solvent silicon with tap water for 6 times. The pH test paper is neutral and the acid value is 0-1 mgKOH / g;

[0040] (4) After vacuum desolventizing of solvent silicon, the solid content is 60% and the yield of silanol is 70%. 2.8 g of zinc isooctanoate is added and the temperature is raised. The condensation reaction is refluxed. When the temperature is maintained at 158° C. and the viscosity of the resin increases significantly and becomes viscous, the resin is cooled and 135 g of propylene glycol methyl ether acetate is added to obtain methyl phenyl silicone resin.

[0041] 2. The resin prepared in Example 1 and various fillers in Table 1 below were put into a preparation tank in proportion, stirred in a sand mill (2000 rpm), filtered, and made into a resin varnish slurry, and then diluted with 20% co-solvent, sprayed on a plate, and the varnish thickness reached 23 μm; after the varnish plate was made, it was baked in an oven at 300 degrees for 10 minutes, and the performance was measured. The performance test is shown in Table 2.

[0042] Table 1 Methyl phenyl silicone resin industrial coating formula composition

[0043] Raw material name Weight(g) Example 1: Methylphenyl silicone resin prepared 65 Defoamer BYK022 0.2 Leveling agent BYK307 0.3 Dispersant BYK190 0.5 Acrylic 1209 14 Xylene 20

[0044] Table 2 Paint film performance test results

[0045]

[0046]

[0047] Example 2

[0048] A method for preparing a methylphenyl silicone resin for a high temperature resistant petroleum pipeline topcoat comprises the following steps:

[0049] (1) First, 150.3 g of monomethyltrichlorosilane, 196.2 g of dimethyldichlorosilane, 443.5 g of monophenyltrichlorosilane, and 760 g of xylene were added to a 3000 ml four-necked flask, and nitrogen was passed through the flask for protection. The mixture A was stirred evenly, and the mixture A was transferred to a constant pressure dropping funnel for standby use;

[0050] (2) Add 350 g of xylene and 3100 g of ionized water into a 5000 ml four-necked flask, start stirring, heat the mixture to 20° C. in a water bath, and slowly add mixture A dropwise at a rate of 1 drop / 1 second; maintain the temperature in the four-necked flask between 20 and 30° C. When the temperature exceeds 27° C., stop heating in the water bath, add ice cubes to cool the mixture to maintain the process temperature at 20-30° C., and continue adding dropwise for 4.5 hours;

[0051] (3) When the addition is completed, continue to maintain the temperature at 25-30°C for half an hour. After the maintenance is completed, let it stand for half an hour, then separate the lower layer of acid water, and wash the upper layer of solvent silicon with tap water for 6 times. The pH test paper is neutral and the acid value is 0-1 mgKOH / g;

[0052] (4) After vacuum desolventizing of solvent silicon, the solid content is 60% and the silanol yield is 74%. 2.9 g of zinc isooctanoate is added and the temperature is raised. The reflux condensation reaction is carried out. When the temperature is maintained at 158° C., the viscosity of the resin increases significantly and becomes viscous. The resin is cooled and 184 g of xylene is added to obtain methylphenyl silicone resin.

[0053] 2. A paint film was prepared according to the same coating formulation as in Table 1 of Example 1, and the performance tests were shown in Table 3 below.

[0054] Table 3 Paint film performance test results

[0055]

[0056]

[0057] Example 3

[0058] A method for preparing a methylphenyl silicone resin for a high temperature resistant petroleum pipeline topcoat comprises the following steps:

[0059] (1) First, 120 g of monomethyltrichlorosilane, 206 g of dimethyldichlorosilane, 358 g of monophenyltrichlorosilane, 126 g of diphenyldichlorosilane, and 1600 g of xylene were added to a 3000 ml four-necked flask, and nitrogen was passed through the flask for protection. The mixture was stirred to obtain a mixture A, and the mixture A was transferred to a constant pressure dropping funnel for standby use;

[0060] (2) Add 1090 g of xylene and 1500 g of ionized water into a 5000 ml four-necked flask, start stirring, heat the mixture to 26° C. in a water bath, and slowly add mixture A dropwise at a rate of 1 drop / 1 second; maintain the temperature in the four-necked flask between 26 and 38° C. When the temperature exceeds 35° C., stop heating in the water bath, add ice cubes to cool the mixture to maintain the process temperature at 26-38° C., and continue adding dropwise for 6 hours;

[0061] (3) When the addition is completed, continue to maintain at 30-35°C for half an hour. After the maintenance is completed, let it stand for half an hour, then separate the lower layer of acid water, and wash the upper layer of solvent silicon with tap water for 6 times. The pH test paper is neutral and the acid value is 0-1 mgKOH / g;

[0062] (4) After vacuum desolventizing of solvent silicon, the solid content was 60% and the silanol yield was 67%. 2.7 g of zinc isooctanoate was added and the temperature was raised. The reflux condensation reaction was carried out. When the temperature was maintained at 158° C., the viscosity of the resin increased significantly. The resin was cooled and 94 g of xylene was added to obtain methylphenyl silicone resin.

[0063] 2. A paint film was prepared according to the same coating formulation as in Table 1 of Example 1, and the performance tests were shown in Table 4 below.

[0064] Table 4 Paint film performance test results:

[0065]

[0066]

[0067] By comparing Example 3 with Example 1, when the amount of diphenyldichlorosilane in Example 3 is doubled, the hardness is increased from 4H to 5H; after xylene replaces propylene glycol methyl ether acetate, its gloss decreases from 118° to 110°, but the self-drying property is reduced; the ionized water is reduced from 2600g to 1500g, the hydrolysis reaction temperature is increased, and the yield decreases by 3%.

[0068] By comparing Example 2 with Example 1, Example 2 does not have the monomer diphenyldichlorosilane, the mass ratio of other monomers is slightly adjusted, and xylene replaces propylene glycol methyl ether acetate. The hardness is reduced from 4H to 2H, the high temperature resistance, impact resistance, adhesion and flexibility are all reduced, and the self-drying property and yield are improved.

[0069] Finally, the self-drying performance of the resin in Example 1 is moderate, the high temperature resistance meets the requirements, and other indicators are also acceptable, which shows that the scientific ratio of each component has achieved a very good and unexpected technical effect.

[0070] The comparison results of the above embodiments show that the different raw materials of each component and the different amounts of the raw materials ultimately lead to significant changes in performance, and the comprehensive performance of embodiment 1 of the present invention is significantly better than that of other embodiments.

[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat, characterized in that: It is made from the following raw materials: Component A: one of monomethyltrichlorosilane, dimethyldichlorosilane, monophenyltrichlorosilane, diphenyldichlorosilane or a combination thereof; Component B: one of toluene, xylene, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, or a combination thereof; Component C: one or a combination of toluene, xylene, acetone, propylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, n-butanol, ionized water, and tap water; Component D: one of zinc octoate, calcium octoate, isopropyl titanate or a combination thereof.

2. The methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 1, characterized in that: It is made of the following raw materials in weight percentage: Component A 12-20%, component B 15-35%, component C 50-70%, component D 0-1%.

3. The methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 1, characterized in that: It is made of the following raw materials in weight percentage: Component A: 16.2%; Component B: 21.6%; Component C: 61.7%; Component D: 0.5%.

4. The methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 1, characterized in that: It is prepared from the following raw materials by weight: 124.5g of monomethyltrichlorosilane, 226.7g of dimethyldichlorosilane, 385.5g of monophenyltrichlorosilane, 73.3g of diphenyldichlorosilane, 1080g of propylene glycol methyl ether acetate, 510g of propylene glycol methyl ether acetate, 2600g of ionized water and 2.8g of zinc isooctanoate.

5. The methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 150.3 g of monomethyltrichlorosilane, 196.2 g of dimethyldichlorosilane, 443.5 g of monophenyltrichlorosilane, 1110 g of xylene, 3100 g of ionized water and 2.9 g of zinc isooctanoate.

6. The methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 120g of monomethyltrichlorosilane, 206g of dimethyldichlorosilane, 358g of monophenyltrichlorosilane, 126g of diphenyldichlorosilane, 2690g of xylene, 1500g of ionized water and 2.7g of zinc isooctanoate.

7. The method for preparing the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) First, add a certain amount of component A and component B into a reaction container, stir evenly to form a mixture A, and transfer the mixture A into a constant pressure dropping funnel for standby use; (2) Add component C into the reaction vessel, start stirring, heat the mixture to 20-30° C. in a water bath, and slowly add the mixture A in step (1) dropwise; continue the addition for 4-6 hours; (3) When the addition is completed, continue to maintain the temperature at 25-33°C for a period of time. When the maintenance is completed, let it stand, then separate the lower layer of acid water, wash the upper layer of solvent silicon with tap water, the pH test paper is neutral, and the acid value is 0-1 mgKOH / g; (4) After the solvent silicon in step (3) is vacuum desolventized, component D is added and the temperature is raised to carry out a reflux condensation reaction. When the viscosity of the resin increases significantly and becomes viscous, it is cooled and a certain amount of component B is added to obtain methylphenyl silicone resin.

8. The method for preparing the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 7, characterized in that: The following steps are involved: (1) First, add a certain amount of component A and component B into a four-necked flask and stir to obtain a mixture A. Transfer the mixture A into a constant pressure dropping funnel and set aside; (2) Add component C to a four-necked flask, start stirring, heat the mixture to 20° C. in a water bath, and slowly drip the mixture A in step (1) at a drip rate of 1 drop / 1 second for 4-6 hours; during the dripping process, the temperature in the four-necked flask is maintained between 20-38° C. When the temperature exceeds 35° C., stop heating in the water bath and maintain the temperature. If the temperature rises rapidly, add ice cubes to cool it down and maintain the process temperature at 23-33° C.; (3) When the addition is completed, continue to maintain the temperature at 25-33°C for half an hour. After the maintenance is completed, let it stand for half an hour, then separate the lower layer of acid water, and wash the upper layer of solvent silicon with tap water 5-6 times. The pH test paper is neutral and the acid value is 0-1 mgKOH / g; (4) After the solvent silicon in step (3) is vacuum desolventized, component D is added, the temperature is raised, and reflux condensation reaction is carried out. When the temperature is maintained at 158° C. and the viscosity of the resin increases significantly and becomes viscous, the resin is cooled and a certain amount of component B is added to obtain methylphenyl silicone resin.

9. The method for preparing the methylphenyl silicone resin for high temperature resistant petroleum pipeline topcoat according to claim 8, characterized in that: After the condensation reaction is completed, add component B when it is cooled to 130°C. After the solid content, viscosity and acid value are qualified, cool it to below 80°C and discharge the material to obtain methylphenyl silicone resin.

Citation Information

Patent Citations

  • Method for preparing high temperature resistant silicone resin

    CN101423611A

  • Methylphenyl silicon resin and preparation method thereof

    CN103755960A

  • Solid polyester modified silicon resin for heat-resisting powder paints and preparation method thereof

    CN107254050A

  • Preparation method for methylphenyl silicone resin and coating

    CN108707231A

  • Preparation method of high-yield methyl phenyl silicone resin

    CN117285711A