Ultrahigh-temperature well cementation spacer fluid system as well as preparation method and application thereof
By optimizing the composition of ultra-high temperature cementing fluid and using specific polymer suspension stabilizers and flushing agents, the problem of insufficient temperature resistance of existing high temperature sealing fluids above 200℃ has been solved, achieving stability and compatibility in an environment of 240℃, thus meeting the cementing requirements of deep and ultra-deep wells.
Patent Information
- Application Number
- CN202310620618.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
Existing high-temperature isolation fluid systems have insufficient temperature resistance above 200℃, which cannot meet the cementing technology requirements of complex deep and ultra-deep wells. Furthermore, their rheological properties and suspension stability are poor, affecting displacement efficiency and cementation quality.
Polymer suspension stabilizers were prepared using 2-acrylamido-2-methylpropanesulfonic acid, N-vinylcaprolactam, 1-vinylimidazole and octadecyldimethylallylammonium chloride as monomers. Combined with a flushing agent composed of surfactants, organic solvents and chelating agents, as well as an anti-fouling agent, the composition of ultra-high temperature cementing and isolation fluid was optimized to ensure stability and compatibility at 240℃.
It achieves good suspension stability and rheological properties at 240℃, has high flushing efficiency, and is compatible with cement slurry and drilling fluid. It is suitable for cementing operations in special wells such as high-temperature and high-pressure gas wells and unconventional oil and gas wells, and improves displacement efficiency and bonding strength.
Smart Images

Figure BDA0004256018450000091 
Figure BDA0004256018450000101 
Figure BDA0004256018450000102
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil and gas well cementing admixtures, and in particular relates to an ultra-high temperature cementing spacer fluid system and a preparation method and application thereof. Background Art
[0002] With the increasing intensity of oil and gas exploration and development, more and more deep and ultra-deep well cementing operations are being carried out. Since such wells require large investments, high risks and high engineering difficulty, spacer fluid plays an important supporting role in ensuring the safety of cementing operations in such wells, avoiding quality and safety accidents and improving the sealing quality of cement slurry. In deep and ultra-deep well cementing applications, the polymer thickening material in the spacer fluid system is prone to molecular chain oxidation and breakage, resulting in a rapid decrease in viscosity and weakened suspension, which changes the properties of the spacer fluid and is difficult to adjust and control, affecting the safety of cementing construction. At the same time, in order to maintain the wellbore pressure balance, the pressure of the liquid column in the well must always be balanced or slightly higher than the formation pressure, and a high-density spacer fluid system must be used. The increase in the density of the spacer fluid will inevitably increase the amount of weighting material, which will in turn cause problems such as poor rheological properties of the slurry. The rheological properties and slurry stability of the spacer fluid system have a great influence on the drilling fluid displacement efficiency, and the drilling fluid displacement efficiency is one of the important guarantee conditions for the success of oil and gas well cementing construction. Therefore, improving the rheological stability of high-temperature and ultra-high-temperature cementing spacer fluid systems plays a vital role in improving displacement efficiency, protecting oil and gas layers, and ensuring the cementing quality of the cement sheath and the second interface, providing technical support for cementing in subsequent oil well operations and increasing reserves and production in oil fields.
[0003] The prior art has disclosed a variety of methods to solve the above problems. CN109135697A discloses a high temperature resistant ultra-high density oil displacement isolation fluid and a preparation method thereof. In parts by weight, the isolation fluid includes: 80 to 245 parts of weighting material, 35 to 60 parts of quartz sand, 4 to 12 parts of microsilica powder, 4 to 15 parts of suspending agent, 5 to 25 parts of surfactant, 0.6 to 1.4 parts of drag reducer, 0.5 parts of defoaming agent, and 100 parts of water. The isolation fluid has good slurry stability and flowability, and can effectively guarantee the oil displacement effect in an oil-wet environment. However, the isolation fluid is only suitable for oil-based drilling fluids in high temperature environments, and its maximum temperature resistance is 200°C.
[0004] CN114426816A discloses a spacer fluid for high temperature resistant cementing and its preparation method and application. The spacer fluid includes a viscosity enhancer, a high temperature suspension stabilizer, a thickening thixotropic agent, a surfactant, a density regulator and water. The high temperature suspension stabilizer includes ultrafine silica, microsilica powder and attapulgite, but ultrafine silica and microsilica powder have adverse effects on the rheological properties of the spacer fluid, and the applicable temperature of the spacer fluid is 30-200°C.
[0005] CN104449606A discloses an isolation fluid for high temperature resistant cementing and a manufacturing method thereof. The isolation fluid is composed of 100 parts by weight of fresh water, 2-8 parts by weight of suspending agent, 2-10 parts by weight of diluent, 25-400 parts by weight of weighting agent, and 1-15 parts by weight of flushing agent. The isolation fluid system has good suspension stability and good rheological properties, is compatible with conventional cement slurry and drilling fluid systems, and can improve displacement efficiency. However, the isolation fluid is only stable under 180°C conditions, and its temperature resistance is insufficient under ultra-high temperature conditions.
[0006] Although the high temperature spacer fluid system in the prior art has good rheological properties and stability, and can improve displacement efficiency, its maximum temperature resistance can only reach 200°C, which cannot meet the ultra-high temperature (above 200°C, bottom hole circulation temperature, BHCT) cementing technical requirements of complex deep wells and ultra-deep wells. Therefore, it is urgent to develop an ultra-high temperature cementing spacer fluid system. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide an ultra-high temperature cementing spacer fluid system and its preparation method and application. The ultra-high temperature cementing spacer fluid system of the present invention can withstand a high temperature of 240°C, has good sedimentation stability, rheological properties and flushing effect, and has good compatibility with commonly used cement slurry and drilling fluid.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides an ultra-high temperature cementing spacer fluid system, which comprises the following components in parts by weight: 100 parts of water, 1-6 parts of a suspension stabilizer, 3-10 parts of a flushing agent, 1-20 parts of an anti-pollution agent, 0.2-0.5 parts of a defoaming agent, and 90-400 parts of a weighting agent;
[0009] The suspension stabilizer comprises a polymer prepared from 2-acrylamide-2-methylpropane sulfonic acid, N-vinyl caprolactam, 1-vinylimidazole and octadecyl dimethyl allyl ammonium chloride as monomers; and the weight ratio of 2-acrylamide-2-methylpropane sulfonic acid, N-vinyl caprolactam, 1-vinylimidazole and octadecyl dimethyl allyl ammonium chloride is (15-25):(15-25):(7-15):(10-15).
[0010] According to a specific embodiment of the present invention, preferably, the ultra-high temperature cementing isolation fluid system includes the following components, measured in parts by weight: 100 parts of water, 2-5 parts of a suspension stabilizer, 3-10 parts of a flushing agent, 3-10 parts of an anti-pollution agent, 0.2-0.5 parts of a defoaming agent, and 90-400 parts of a weighting agent.
[0011] In the above-mentioned ultra-high temperature cementing spacer fluid system, preferably, the suspension stabilizer is prepared by at least the following steps: dissolving 2-acrylamide-2-methylpropanesulfonic acid, N-vinyl caprolactam, 1-vinyl imidazole, and octadecyl dimethyl allyl ammonium chloride in a weight ratio of (15-25):(15-25):(7-15):(10-15) in an appropriate amount of water to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 6.5-7.5 to obtain a second mixed solution; and then adding an initiator to the second mixed solution to carry out a polymerization reaction. After the reaction is completed, a polymer solution is obtained, which is the suspension stabilizer.
[0012] In some specific embodiments of the present invention, preferably, the weight ratio of 2-acrylamide-2-methylpropanesulfonic acid, N-vinylcaprolactam, 1-vinylimidazole, octadecyldimethylallylammonium chloride and water is (15-25):(15-25):(7-15):(10-15):(200-350).
[0013] In some specific embodiments of the present invention, preferably, sodium hydroxide is used to adjust the pH value of the first mixed solution to 6.5-7.5.
[0014] In some specific embodiments of the present invention, preferably, the initiator comprises ammonium persulfate and sodium bisulfite. More preferably, based on the total weight of the second mixed solution being 100%, the amount of ammonium persulfate added is 0.4-0.8%, and the amount of sodium bisulfite added is 0.1-0.3%.
[0015] In some specific embodiments of the present invention, preferably, the polymerization reaction temperature is 50-70° C. and the time is 2-5 hours.
[0016] In the above-mentioned ultra-high temperature cementing isolation fluid system, preferably, the flushing agent comprises a mixture of a surfactant, an organic solvent and a chelating agent in a weight ratio of (20-35):(50-70):(10-15).
[0017] In some specific embodiments of the present invention, preferably, the surfactant includes one or a combination of lauryl glucoside, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate.
[0018] In some specific embodiments of the present invention, preferably, the organic solvent includes n-butanol or the like.
[0019] In some specific embodiments of the present invention, preferably, the chelating agent includes disodium ethylenediaminetetraacetate and / or tetrasodium ethylenediaminetetraacetate, etc.
[0020] In some specific embodiments of the present invention, the surfactant, the organic solvent, and the chelating agent are uniformly mixed according to the above ratio to prepare the flushing agent of the present invention.
[0021] In the above-mentioned ultra-high temperature cementing spacer fluid system, preferably, the anti-pollution agent comprises a mixture of a first anti-pollution agent and a second anti-pollution agent in a weight ratio of (40-80): (5-30), the first anti-pollution agent comprises one or a combination of ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, polyaminopolyether methylenephosphonic acid, aminotrimethylenephosphonic acid and hydrolyzed polymaleic anhydride, etc., and the second anti-pollution agent comprises sodium gluconate and / or sodium tripolyphosphate, etc. More preferably, the first anti-pollution agent is selected from one or two of ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, polyaminopolyether methylenephosphonic acid, aminotrimethylenephosphonic acid and hydrolyzed polymaleic anhydride, and the second anti-pollution agent is selected from one of sodium gluconate and sodium tripolyphosphate.
[0022] In some specific embodiments of the present invention, the first anti-pollution agent and the second anti-pollution agent are uniformly mixed according to the above ratio to prepare the anti-pollution agent of the present invention.
[0023] In the above-mentioned ultra-high temperature cementing spacer fluid system, preferably, the defoaming agent includes one or a combination of tributyl phosphate, polyoxypropylene glycerol ether and polydimethylsiloxane.
[0024] In the above-mentioned ultra-high temperature cementing spacer fluid system, preferably, the weighting agent includes one or a combination of barite powder, hematite powder, iron ore powder and the like.
[0025] The second aspect of the present invention provides a method for preparing the ultra-high temperature cementing spacer fluid system, which comprises the following steps:
[0026] 1-6 parts by weight (preferably 2-5 parts by weight) of a suspension stabilizer is added to 100 parts by weight of water and stirred for a period of time; then 90-400 parts by weight of a weighting agent, 3-10 parts by weight of a flushing agent, and 1-20 parts by weight (preferably 3-10 parts by weight) of an anti-pollution agent are added and stirred for a period of time; then 0.2-0.5 parts by weight of a defoaming agent is added to obtain the ultra-high temperature cementing isolation fluid system.
[0027] In the above preparation method, preferably, the stirring speed after adding the suspension stabilizer into water is 2000 r / min±500 r / min.
[0028] In the above preparation method, preferably, the time for stirring after adding the suspension stabilizer into water is 1-5 minutes.
[0029] In the above preparation method, preferably, the stirring speed after adding the weighting agent, the flushing agent and the anti-pollution agent is 2000 r / min±500 r / min.
[0030] In the above preparation method, preferably, the stirring time after adding the weighting agent, flushing agent and anti-pollution agent is 2-10 minutes.
[0031] The third aspect of the present invention provides the use of the above-mentioned ultra-high temperature cementing spacer fluid system in cementing operations of special wells.
[0032] In the above-mentioned applications, preferably, the special wells include high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, ultra-deep wells, etc.
[0033] In the above application, preferably, the bottom hole circulation temperature of the special well is below 240°C, more preferably 90-240°C.
[0034] The technical solution of the present invention has at least the following beneficial technical effects:
[0035] (1) Based on the suspension stabilization mechanism of the ultra-high temperature cementing spacer fluid system, the present invention uses 2-acrylamide-2-methylpropane sulfonic acid, N-vinyl caprolactam, 1-vinylimidazole and octadecyl dimethyl allyl ammonium chloride as monomers, optimizes the design of the polymer main chain and side chain, and synthesizes a new type of tetrapolymer suspension stabilizer with a temperature resistance of up to 240°C and good high-temperature suspension stabilization effect.
[0036] (2) The anti-pollution agent of the present invention can promote compatibility between fluids, effectively preventing the problem that the engineering performance does not meet the construction requirements due to contamination between fluids. The ultra-high temperature cementing spacer fluid system of the present invention has good compatibility with commonly used cement slurry and drilling fluid, and is not prone to downhole fluid contamination.
[0037] (3) The flushing agent of the present invention is composed of a surfactant, an organic solvent and a chelating agent, which plays a decisive role in improving the flushing efficiency of the spacer fluid system. The flushing efficiency of the ultra-high temperature cementing spacer fluid system of the present invention is higher than 90%, which is beneficial to improve the flushing efficiency of the drilling fluid and well wall mud cake adhered to the casing wall, improve the interface bonding state, and increase the bonding strength between the interface and cement stone, and has a good oil displacement effect.
[0038] (4) The ultra-high temperature cementing spacer fluid system of the present invention is suitable for an environment of 90-240°C (BHCT) and can withstand a high temperature of 240°C. Under the condition of 240°C, the upper and lower density difference of the ultra-high temperature cementing spacer fluid system can be controlled within 0.1 g / cm 3 The viscosity rebound value at the moment of restarting after stopping for 30 minutes is less than 40Bc, and the suspension stability is good.
[0039] (5) The ultra-high temperature cementing spacer fluid system of the present invention has strong adaptability and stable performance, and can meet the cementing technical requirements of special wells such as high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, and ultra-deep wells.
[0040] In summary, the present invention provides an ultra-high temperature cementing spacer fluid system and its preparation method and application. The ultra-high temperature cementing spacer fluid system is suitable for 90-240℃ environment (BHCT), and its sedimentation stability can be controlled at 0.1g / cm 3 It has good rheological properties and flushing effects, and can improve the bonding properties between the cement sheath and the first and second interfaces of cementing. It also has good compatibility with commonly used cement slurries and drilling fluids, and can meet the cementing technology requirements of special wells such as deep wells and ultra-deep wells with a bottom hole circulation temperature of 240°C. DETAILED DESCRIPTION
[0041] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0042] Example 1
[0043] The present embodiment provides an ultra-high temperature cementing isolation fluid system, which includes the following components, in parts by weight: 100 parts of water, 3 parts of a suspension stabilizer, 10 parts of a flushing agent, 3 parts of an anti-pollution agent, 0.2 parts of a defoaming agent, and 90 parts of a weighting agent.
[0044] The suspension stabilizer is prepared by the following steps:
[0045] In parts by weight, 20.7 parts of 2-acrylamide-2-methylpropanesulfonic acid, 19.8 parts of N-vinyl caprolactam, 9.4 parts of 1-vinylimidazole and 10 parts of octadecyl dimethyl allyl ammonium chloride are dissolved in 264 parts of deionized water to obtain a first mixed solution, in which the total monomer concentration is 18.5wt.%; sodium hydroxide is added to the first mixed solution to adjust the pH value to 7 to obtain a second mixed solution; the second mixed solution is poured into a three-necked flask, mixed and stirred for about 15 minutes, and then 0.5% of ammonium persulfate and 0.1% of sodium bisulfite accounting for the total weight of the second mixed solution are added, and the mixture is heated to 60°C for polymerization reaction for 3 hours. After the reaction is completed, a polymer solution is obtained, which is the suspension stabilizer.
[0046] The flushing agent is a mixture of a composite surfactant, an organic solvent and a chelating agent in a weight ratio of 30:60:10. The composite surfactant is lauryl glucoside and fatty alcohol polyoxyethylene ether AEO-9 in a weight ratio of 1:1. The organic solvent is n-butanol. The chelating agent is disodium ethylenediaminetetraacetate. The composite surfactant, the organic solvent and the chelating agent are uniformly mixed according to a proportion to prepare the flushing agent.
[0047] The anti-pollution agent is a mixture of hydrolyzed polymaleic anhydride and sodium tripolyphosphate in a weight ratio of 70:5. The anti-pollution agent can be prepared by uniformly mixing the hydrolyzed polymaleic anhydride and sodium tripolyphosphate according to a certain proportion.
[0048] The defoamer is tributyl phosphate.
[0049] The weighting agent is barite powder (density 4.2g / cm 3 , particle size is 20μm).
[0050] The ultra-high temperature cementing spacer fluid system of the present embodiment is prepared by the following steps: pouring 100 parts by weight of water into a stirring slurry cup, slowly adding 3 parts by weight of a suspension stabilizer under stirring conditions, and then stirring at a speed of 2000 r / min for 1 min in a Waring stirrer, and then slowly adding 90 parts by weight of a weighting agent, 10 parts by weight of a flushing agent, and 3 parts by weight of an anti-pollution agent, and then stirring at a speed of 2000 r / min for 3 min, and finally adding 0.2 parts by weight of a defoaming agent, stirring evenly, to obtain the ultra-high temperature cementing spacer fluid system of the present embodiment.
[0051] The density of the ultra-high temperature cementing spacer fluid system in this embodiment is 1.50 g / cm 3 .
[0052] Example 2
[0053] The present embodiment provides an ultra-high temperature cementing isolation fluid system, which includes the following components, in parts by weight: 100 parts of water, 4 parts of a suspension stabilizer, 10 parts of a flushing agent, 3 parts of an anti-pollution agent, 0.2 parts of a defoaming agent, and 188 parts of a weighting agent.
[0054] The suspension stabilizer, flushing agent, anti-pollution agent, defoaming agent and weighting agent used in this embodiment are the same as those in Example 1.
[0055] The ultra-high temperature cementing spacer fluid system of the present embodiment is prepared by the following steps: pouring 100 parts by weight of water into a stirring slurry cup, slowly adding 4 parts by weight of a suspension stabilizer under stirring conditions, and then stirring at a speed of 2000 r / min for 1 min in a Waring stirrer, and then slowly adding 188 parts by weight of a weighting agent, 10 parts by weight of a flushing agent, and 3 parts by weight of an anti-pollution agent, and then stirring at a speed of 2000 r / min for 3 min, and finally adding 0.2 parts by weight of a defoaming agent, stirring evenly, to obtain the ultra-high temperature cementing spacer fluid system of the present embodiment.
[0056] The density of the ultra-high temperature cementing spacer fluid system of this embodiment is 1.90 g / cm 3 .
[0057] Example 3
[0058] The present embodiment provides an ultra-high temperature cementing isolation fluid system, which includes the following components, in parts by weight: 100 parts of water, 5 parts of a suspension stabilizer, 10 parts of a flushing agent, 3 parts of an anti-pollution agent, 0.2 parts of a defoaming agent, and 293 parts of a weighting agent.
[0059] The suspension stabilizer, flushing agent, anti-pollution agent, defoaming agent and weighting agent used in this embodiment are the same as those in Example 1.
[0060] The ultra-high temperature cementing spacer fluid system of the present embodiment is prepared by the following steps: pouring 100 parts by weight of water into a stirring slurry cup, slowly adding 5 parts by weight of a suspension stabilizer under stirring conditions, and then stirring at a speed of 2000 r / min for 1 min in a Waring stirrer, and then slowly adding 293 parts by weight of a weighting agent, 10 parts by weight of a flushing agent, and 3 parts by weight of an anti-pollution agent, and then stirring at a speed of 2000 r / min for 3 min, and finally adding 0.2 parts by weight of a defoaming agent, stirring evenly, to obtain the ultra-high temperature cementing spacer fluid system of the present embodiment.
[0061] The density of the ultra-high temperature cementing spacer fluid system in this embodiment is 2.20 g / cm 3 .
[0062] Comparative Example 1
[0063] This comparative example provides a cementing spacer fluid system. The cementing spacer fluid system is substantially the same as the ultra-high temperature cementing spacer fluid system provided in Example 1, except that bentonite is used as a suspension stabilizer in this comparative example.
[0064] In parts by weight, the cementing isolation fluid system of this comparative example includes the following components: 100 parts of water, 3 parts of suspension stabilizer, 10 parts of flushing agent, 3 parts of anti-pollution agent, 0.2 parts of defoaming agent and 90 parts of weighting agent.
[0065] The flushing agent, anti-pollution agent, defoaming agent and weighting agent used in this comparative example are the same as those in Example 1. The preparation method of the cementing spacer fluid system in this comparative example is also the same as that in Example 1.
[0066] The density of the cementing spacer fluid system in this comparative example is 1.50 g / cm 3 .
[0067] Comparative Example 2
[0068] This comparative example provides a cementing spacer fluid system. The cementing spacer fluid system is substantially the same as the ultra-high temperature cementing spacer fluid system provided in Example 2, except that: this comparative example does not use an anti-pollution agent.
[0069] In parts by weight, the cementing isolation fluid system of this comparative example includes the following components: 100 parts of water, 4 parts of a suspension stabilizer, 10 parts of a flushing agent, 0.2 parts of a defoaming agent, and 188 parts of a weighting agent.
[0070] The suspension stabilizer, flushing agent, defoaming agent and weighting agent used in this comparative example are the same as those in Example 1.
[0071] The cementing spacer fluid system of this comparative example is prepared by the following steps: pouring 100 parts by weight of water into a stirring slurry cup, slowly adding 4 parts by weight of a suspension stabilizer under stirring conditions, and then stirring at a speed of 2000 r / min for 1 min in a Waring stirrer, and then slowly adding 188 parts by weight of a weighting agent and 10 parts by weight of a flushing agent, and then stirring at a speed of 2000 r / min for 3 min, and finally adding 0.2 parts by weight of a defoaming agent, stirring evenly, to obtain the cementing spacer fluid system of this comparative example.
[0072] The density of the cementing spacer fluid system in this comparative example is 1.90 g / cm 3 .
[0073] Comparative Example 3
[0074] This comparative example provides a cementing spacer fluid system. The cementing spacer fluid system is substantially the same as the ultra-high temperature cementing spacer fluid system provided in Example 3, except that: this comparative example does not use a flushing agent.
[0075] In parts by weight, the cementing isolation fluid system of this comparative example includes the following components: 100 parts of water, 5 parts of a suspension stabilizer, 3 parts of an anti-pollution agent, 0.2 parts of a defoaming agent, and 270 parts of a weighting agent.
[0076] The suspension stabilizer, anti-pollution agent, defoaming agent and weighting agent used in this comparative example are the same as those in Example 1.
[0077] The cementing isolation fluid system of this comparative example is prepared by the following steps: pouring 100 parts by weight of water into a stirring slurry cup, slowly adding 5 parts by weight of a suspension stabilizer under stirring conditions, and then stirring at a speed of 2000 r / min for 1 min in a Waring stirrer, and then slowly adding 270 parts by weight of a weighting agent and 3 parts by weight of an anti-pollution agent, and then stirring at a speed of 2000 r / min for 3 min, and finally adding 0.2 parts by weight of a defoaming agent, stirring evenly, to obtain the cementing isolation fluid system of this comparative example.
[0078] The density of the cementing spacer fluid system in this comparative example is 2.20 g / cm 3 .
[0079] Comparative Example 4
[0080] This comparative example provides a cementing spacer fluid system. The cementing spacer fluid system is substantially the same as the ultrahigh temperature cementing spacer fluid system provided in Example 1, except that the suspension stabilizer in this comparative example does not use 1-vinylimidazole as one of the monomers.
[0081] The suspension stabilizer of this comparative example is prepared by the following steps:
[0082] In parts by weight, 20.7 parts of 2-acrylamide-2-methylpropanesulfonic acid, 19.8 parts of N-vinyl caprolactam and 10 parts of octadecyl dimethyl allyl ammonium chloride are dissolved in 222 parts of deionized water to obtain a first mixed solution, in which the total monomer concentration is 18.5wt.%; sodium hydroxide is added to the first mixed solution to adjust the pH value to 7 to obtain a second mixed solution; the second mixed solution is poured into a three-necked flask, mixed and stirred for about 15 minutes, and then 0.5% of ammonium persulfate accounting for the total weight of the second mixed solution and 0.1% of sodium bisulfite accounting for the total weight of the second mixed solution are added, and the mixture is heated to 60°C for polymerization reaction for 3 hours. After the reaction is completed, a polymer solution is obtained, which is the suspension stabilizer.
[0083] In parts by weight, the cementing isolation fluid system of this comparative example includes the following components: 100 parts of water, 3 parts of suspension stabilizer, 10 parts of flushing agent, 3 parts of anti-pollution agent, 0.2 parts of defoaming agent and 90 parts of weighting agent.
[0084] The flushing agent, anti-pollution agent, defoaming agent and weighting agent used in this comparative example are the same as those in Example 1. The preparation method of the cementing spacer fluid system in this comparative example is also the same as that in Example 1.
[0085] The density of the cementing spacer fluid system in this comparative example is 1.50 g / cm 3 .
[0086] Comparative Example 5
[0087] This comparative example provides a cementing spacer fluid system. The cementing spacer fluid system is substantially the same as the ultra-high temperature cementing spacer fluid system provided in Example 2, except that: this comparative example uses hydrolyzed polymaleic anhydride as an anti-pollution agent.
[0088] In parts by weight, the cementing isolation fluid system of this comparative example includes the following components: 100 parts of water, 4 parts of suspension stabilizer, 10 parts of flushing agent, 3 parts of anti-pollution agent, 0.2 parts of defoaming agent and 188 parts of weighting agent.
[0089] The suspension stabilizer, flushing agent, defoaming agent and weighting agent used in this comparative example are the same as those in Example 2. The preparation method of the cementing spacer fluid system in this comparative example is also the same as that in Example 2.
[0090] The density of the cementing spacer fluid system in this comparative example is 1.90 g / cm 3 .
[0091] Test Example 1 Rheological properties of ultra-high temperature cementing spacer fluid system at 90-240℃
[0092] The densities provided in Examples 1 to 3 are 1.50 g / cm 3 , 1.90g / cm 3 , 2.20g / cm 3 The ultra-high temperature cementing spacer fluid system was tested for its rheological properties at 90-240°C. The rheological properties of the spacer fluid system were tested according to the method described in GB / T19139-2012 "Test Methods for Oil Well Cement", and the test results are shown in Table 1.
[0093] Table 1 Rheological properties of ultra-high temperature cementing spacer fluid system at 90-240℃
[0094]
[0095]
[0096] It can be seen from Table 1 that the spacer fluid systems of different densities prepared in Examples 1 to 3 all have good suspension performance. As the temperature increases, the apparent viscosity of the spacer fluid systems decreases to varying degrees, but even at 240°C, the apparent viscosity is greater than 30 mPa·s. It can be seen that the ultra-high temperature cementing spacer fluid systems prepared in Examples 1 to 3 have good high-temperature suspension stability.
[0097] Test Example 2: Sedimentation stability performance of ultra-high temperature cementing spacer fluid system
[0098] The densities provided in Examples 1 to 3 are 1.50 g / cm 3 , 1.90g / cm3 , 2.20g / cm 3 The ultra-high temperature cementing spacer fluid system was tested for its sedimentation stability at 90-240°C. The sedimentation stability of the spacer fluid system was tested according to the method described in GB / T19139-2012 "Test Methods for Oil Well Cement", and the test results are shown in Table 2, Table 3, and Table 4.
[0099] Table 2 Sedimentation stability performance of the ultra-high temperature cementing spacer fluid system of Example 1 at 90-240°C
[0100]
[0101] Table 3 Sedimentation stability performance of the ultra-high temperature cementing spacer fluid system of Example 2 at 90-240°C
[0102]
[0103] Table 4 Sedimentation stability performance of the ultra-high temperature cementing spacer fluid system of Example 3 at 90-240°C
[0104]
[0105] It can be seen from Tables 2 to 4 that the isolation liquid systems of different densities prepared in Examples 1 to 3 all have good suspension stability at high temperatures. At 210°C, the density is 1.50 g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.026g / cm 3 , its plastic viscosity is 29mPa·s; density is 1.90g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.033g / cm 3 Its plastic viscosity is 45mPa·s; its density is 2.20g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.038g / cm 3 , its plastic viscosity is 53mPa·s. At 240℃, its density is 1.50g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.043g / cm 3 , its plastic viscosity is 26mPa·s; density is 1.90g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.051g / cm 3 Its plastic viscosity is 40mPa·s; its density is 2.20g / cm 3 The density difference between the upper and lower density of the isolation liquid system is 0.065g / cm 3, and its plastic viscosity is 52mPa·s. Under the condition of 90-240°C, the spacer fluid systems of different densities prepared in Examples 1 to 3 all meet the requirements of on-site construction. It can be seen that the ultra-high temperature cementing spacer fluid systems prepared in Examples 1 to 3 have good temperature resistance and rheological properties.
[0106] As shown in Tables 2 to 4, this test example examines the instantaneous viscosity change of the isolation fluid systems of different densities prepared in Examples 1 to 3 after being stopped for 30 minutes under different temperature conditions to study their sedimentation stability performance. If the instantaneous viscosity recoil value of startup is greater than 40Bc, the fluid pumping pressure will be greatly increased, and there is a risk of leaking the formation; if it is lower than 40Bc, the sedimentation stability of the isolation fluid system is considered to be good. It can be seen from Tables 2 to 4 that the consistency values of the isolation fluid systems of different densities prepared in Examples 1 to 3 after being stopped for 30 minutes under different temperature conditions are all lower than 40Bc, meeting the performance requirements of cementing engineering.
[0107] Test Example 3 Compatibility of Ultra-High Temperature Cementing Spacer Fluid System with Drilling Fluid and Cement Slurry
[0108] The compatibility test of the spacer fluid system is carried out according to the contents recorded in Chapter 16 of GB / T 19139-2012 "Test Methods for Oil Well Cement". The cement slurry, drilling fluid and spacer fluid system are mixed in different proportions and subjected to high temperature and high pressure thickening tests to test the compatibility of the cement slurry, drilling fluid and spacer fluid system.
[0109] In this test example, the spacer fluid system used is the ultra-high temperature cementing spacer fluid system prepared in Example 2, and its density is 1.90 g / cm 3 .
[0110] The cement slurry used includes the following components: Jiahua G-grade oil well cement (HSR) + 25% 200 mesh quartz sand + 25% 600 mesh quartz sand + 2% microsilicon + 1% dispersant DRS-1S + 5% high temperature reinforcing material DRB-3S + 5% retarder DRH-2L + 5% liquid fluid loss agent DRF-2L + 2% suspension stabilizer DRK-3S + 46% water, where "%" is the weight percentage calculated based on the total weight of Jiahua G-grade oil well cement (HSR). Jiahua G-grade oil well cement is a product of Jiahua Special Cement Co., Ltd., and the remaining materials are products of China National Petroleum Corporation Engineering Technology Research Institute Co., Ltd. The density of the cement slurry is 1.95g / cm 3 .
[0111] The drilling fluid used is a polysulfone drilling fluid, which includes the following components: water + 2% high temperature resistant viscosity enhancer and shearing agent Visco1 + 0.5% NaOH + 3% high temperature resistant and salt resistant fluid loss reducer Redu200 + 3% sulfonated phenolic resin SMP + 3% lignite resin SPNH + 3% sulfonated asphalt FT-1 + 2% polyol PGCS-1 + 2% anti-ultra-high temperature lubricant LUBS50 + 0.5% surfactant OME-2 + 7% potassium chloride + 89% barite, where "%" is the weight percentage calculated based on the total weight of water. The high temperature resistant viscosity enhancer and shearing agent Visco1, the high temperature resistant and salt resistant fluid loss reducer Redu200, the polyol PGCS-1 and the anti-ultra-high temperature lubricant LUBS50 were purchased from Beijing Peikang Jiaye Technology Development Co., Ltd.; the sulfonated phenolic resin SMP, the lignite resin SPNH, the sulfonated asphalt FT-1 and the surfactant OME-2 were purchased from Shandong Deshunyuan Petroleum Technology Co., Ltd. The density of the drilling fluid is 1.56g / cm 3 .
[0112] According to the volume percentage of cement slurry, drilling fluid and spacer fluid in Table 5, two or three fluids are mixed to obtain a mixed slurry. The mixed slurry is subjected to high temperature and high pressure thickening tests at 90°C×35Mpa, 150°C×65Mpa, 210°C×90Mpa and 240°C×100Mpa, respectively. The results are shown in Table 5.
[0113] Table 5 Thickening test results of mixed slurry of cement slurry, drilling fluid and spacer fluid system
[0114]
[0115]
[0116] It can be seen from Table 5 that as the temperature increases, the thickening time of the cement slurry is relatively shortened. When the volume ratio of cement slurry to drilling fluid is 1:1, flocculation occurs in the four groups of mixed slurries under different test conditions. When the cement slurry, drilling fluid and the spacer fluid system prepared in Example 2 are mixed, the thickening time of the slurry is extended. At 240°C, the thickening time of the mixed slurry is greater than 300 minutes. It can be seen that the ultra-high temperature cementing spacer fluid system prepared in Example 2 has good chemical compatibility with drilling fluid and cement slurry, and has strong anti-pollution ability, which can ensure the safety of cement slurry replacement and cementing construction, and meet the needs of high temperature and ultra-high temperature deep well cementing.
[0117] Test Example 4 Flushing Efficiency of Ultra-High Temperature Cementing Spacer Fluid System
[0118] The density provided by Examples 1 to 3 was tested to be 1.50 g / cm 3 , 1.90g / cm 3 , 2.20g / cm3 The flushing efficiency of the ultra-high temperature cementing spacer fluid system is measured by a six-speed rotary viscometer, with the rotation speed set at 200 r / min. The polysulfone drilling fluid used is the same as that in Test Example 3.
[0119] The specific measurement method includes: removing the rotating outer cylinder of the six-speed rotation viscometer, weighing its mass, recorded as W0, rotating the outer cylinder in the drilling fluid at a speed of 200 r / min for 10 minutes so that its outer wall is covered with drilling fluid, letting it stand for 1 minute, and then weighing its mass, recorded as W1; then, filling the measuring cup with isolation fluid, immersing the outer cylinder of the six-speed rotation viscometer covered with drilling fluid in the isolation fluid, rinsing it at a speed of 200 r / min for a few minutes (the specific rinsing time is described below), letting it stand for 1 minute, and weighing the mass of the outer cylinder, recorded as W2.
[0120] The flushing efficiency η is calculated according to the following formula. Three groups of parallel tests are carried out to obtain the average value. The error between parallel tests shall not exceed 5%.
[0121]
[0122] Where: η is flushing efficiency; W0 is the mass of the outer cylinder of the six-speed rotary viscometer, in grams (g); W1 is the mass of the outer cylinder of the six-speed rotary viscometer after being filled with drilling fluid, in grams (g); W2 is the mass of the outer cylinder of the six-speed rotary viscometer after flushing, in grams (g).
[0123] The results are as follows: The flushing time of the ultra-high temperature cementing spacer fluid system prepared in Example 1 is 4.5 minutes, and the flushing efficiency is 100%. The flushing time of the ultra-high temperature cementing spacer fluid system prepared in Example 2 is 4 minutes, and the flushing efficiency is 100%. The flushing time of the ultra-high temperature cementing spacer fluid system prepared in Example 3 is 4 minutes, and the flushing efficiency is 100%. It can be seen that the ultra-high temperature cementing spacer fluid systems prepared in Examples 1 to 3 have high flushing efficiency and meet the cementing technical requirements.
[0124] Test Example 5 Comparison of Sedimentation Stability of Isolation Liquid Systems of Example 1 and Comparative Example 1
[0125] The sedimentation stability performance of the spacer fluid system provided in Example 1 and Comparative Example 1 at 90-240° C. was tested according to the method described in GB / T19139-2012 “Test Methods for Oil Well Cement”. The test results are shown in Table 6.
[0126] Table 6 Sedimentation stability performance of Example 1 and Comparative Example 1 at 90-240°C
[0127]
[0128] The spacer liquid systems of Example 1 and Comparative Example 1 use different suspension stabilizers. The suspension stabilizer in Comparative Example 1 is conventional bentonite on the market, and the suspension stabilizer in Example 1 is the tetrapolymer suspension stabilizer of the present invention. As can be seen from Table 6, the spacer liquid system of Comparative Example 1 has good suspension stability in a temperature environment of 150°C or below, but its suspension stability decreases after exceeding 150°C. The high-temperature dilution phenomenon of the spacer liquid system is more serious, and the sedimentation stability does not meet the requirements of on-site construction. The upper and lower density differences at 210°C and 240°C are both greater than 0.1g / cm 3 This shows that the suspension stabilizer of the present invention has stronger temperature resistance and good high temperature stability compared with conventional suspension stabilizers on the market. The temperature resistance of the suspension stabilizer of the present invention reaches 240°C, while the temperature resistance of conventional suspension stabilizers is only 150°C.
[0129] Test Example 6 Comparison of the compatibility of the spacer fluid system of Example 2 and Comparative Example 2 with cement slurry and drilling fluid
[0130] The compatibility test of the spacer fluid system is carried out according to the contents recorded in Chapter 16 of GB / T 19139-2012 "Test Methods for Oil Well Cement". The cement slurry, drilling fluid and spacer fluid system are mixed in different proportions and subjected to high temperature and high pressure thickening tests to test the compatibility of the cement slurry, drilling fluid and spacer fluid system.
[0131] In this test example, the cement slurry and drilling fluid used are the same as those in Test Example 3. The spacer fluid system used includes the spacer fluid system prepared in Example 2 and Comparative Example 2, and the density of each of them is 1.90 / cm 3 The difference between the isolation liquid system of Comparative Example 2 and Example 2 is that the anti-pollution agent of the present invention is not added to Comparative Example 2.
[0132] According to the volume percentage of cement slurry, drilling fluid and spacer fluid in Table 7, two or three fluids are mixed to obtain a mixed slurry. The mixed slurry is subjected to high temperature and high pressure thickening tests at 90°C×35Mpa, 150°C×65Mpa, 210°C×90Mpa and 240°C×100Mpa, respectively. The results are shown in Table 7.
[0133] Table 7 Thickening test results of mixed slurry of cement slurry, drilling fluid and spacer fluid system
[0134]
[0135]
[0136] It can be seen from Table 7 that as the temperature increases, the thickening time of the cement slurry is relatively shortened. When the volume ratio of cement slurry to drilling fluid is 1:1, the mixed slurries mixed with the spacer fluid system of Example 2 and Comparative Example 2 respectively show flocculation. When the cement slurry, drilling fluid and the spacer fluid system prepared in Example 2 are mixed, the thickening time of the slurry is extended. At 240°C, the thickening time of the mixed slurry is greater than 300min. It can be seen that the ultra-high temperature cementing spacer fluid system prepared in Example 2 has good chemical compatibility with drilling fluid and cement slurry. When the cement slurry, drilling fluid and the spacer fluid system prepared in Comparative Example 2 are mixed, the thickening time of the slurry is shortened to varying degrees. It can be seen that the anti-pollution ability of Comparative Example 2 is poor and does not meet the construction requirements. This shows that the anti-pollution agent of the present invention plays an important role in promoting the three-phase compatibility of cement slurry, drilling fluid and spacer fluid. The spacer fluid system of the present invention can avoid contact pollution of cement slurry and drilling fluid and ensure the safety of cementing construction.
[0137] Test Example 7 Comparison of Flushing Efficiency of Isolation Liquid Systems of Example 3 and Comparative Example 3
[0138] The density provided by Example 3 and Comparative Example 3 was tested according to the method in Test Example 4, and both were 2.20 g / cm 3 The flushing efficiency of the isolation fluid system. The difference between the isolation fluid system of Example 3 and Comparative Example 3 is that the flushing agent of the present invention is not added to Comparative Example 3. The results are: the flushing time of the ultra-high temperature cementing isolation fluid system prepared in Example 3 is 4 minutes, and the flushing efficiency is 100%; while the flushing time of the isolation fluid system prepared in Comparative Example 3 is 5 minutes, and the flushing efficiency is 89%. This shows that the flushing agent of the present invention has a good flushing effect, so that the oil displacement of the isolation fluid system of the present invention is better, the flushing time is short and the flushing efficiency is greater than 90%.
[0139] Test Example 8 Comparison of Sedimentation Stability of Isolation Liquid Systems of Example 1 and Comparative Example 4
[0140] The sedimentation stability performance of the spacer fluid system provided in Example 1 and Comparative Example 4 at 90-240° C. was tested according to the method described in GB / T19139-2012 “Test Methods for Oil Well Cement”. The test results are shown in Table 8.
[0141] Table 8 Sedimentation stability performance of Example 1 and Comparative Example 4 at 90-240°C
[0142]
[0143] The spacer liquid systems of Example 1 and Comparative Example 4 use different suspension stabilizers. The suspension stabilizer in Comparative Example 4 does not use 1-vinylimidazole as one of the monomers. The suspension stabilizer in Example 1 is the tetrapolymer suspension stabilizer of the present invention. The density of the spacer liquid systems prepared in Example 1 and Comparative Example 4 is 1.50 g / cm 3 .
[0144] It can be seen from Table 8 that the isolation liquid system of Comparative Example 4 has good suspension stability in a temperature environment of 150°C and below, but its suspension stability decreases after exceeding 150°C. The high-temperature dilution phenomenon of the isolation liquid system is more serious, and the sedimentation stability does not meet the requirements of on-site construction. The upper and lower density differences at 210°C and 240°C are both greater than 0.1g / cm 3 This shows that the present invention uses 1-vinylimidazole as one of the monomers of the copolymer suspension stabilizer, which plays a key role in improving the temperature resistance and high temperature stability of the suspension stabilizer.
[0145] Test Example 9 Comparison of the compatibility of the spacer fluid system of Example 2 and Comparative Example 5 with cement slurry and drilling fluid
[0146] The compatibility test of the spacer fluid system is carried out according to the contents recorded in Chapter 16 of GB / T 19139-2012 "Test Methods for Oil Well Cement". The cement slurry, drilling fluid and spacer fluid system are mixed in different proportions and subjected to high temperature and high pressure thickening tests to test the compatibility of the cement slurry, drilling fluid and spacer fluid system.
[0147] In this test example, the cement slurry and drilling fluid used are the same as those in Test Example 3. The spacer fluid system used includes the spacer fluid system prepared in Example 2 and Comparative Example 5, and the density of each of them is 1.90 / cm 3 The difference between the isolation liquid system of Comparative Example 5 and Example 2 is that the anti-pollution agent of Comparative Example 5 uses hydrolyzed polymaleic anhydride as the anti-pollution agent, while the anti-pollution agent of Example 2 is a mixture of hydrolyzed polymaleic anhydride and sodium tripolyphosphate.
[0148] According to the volume percentage of cement slurry, drilling fluid and spacer fluid in Table 9, two or three fluids are mixed to obtain a mixed slurry. The mixed slurry is subjected to high temperature and high pressure thickening tests at 90°C×35Mpa, 150°C×65Mpa, 210°C×90Mpa and 240°C×100Mpa, respectively. The results are shown in Table 9.
[0149] Table 9 Thickening test results of mixed slurry of cement slurry, drilling fluid and spacer fluid system
[0150]
[0151]
[0152]
[0153] It can be seen from Table 9 that as the temperature increases, the thickening time of the cement slurry is relatively shortened. When the volume ratio of cement slurry to drilling fluid is 1:1, the mixed slurries mixed with the spacer fluid system of Example 2 and Comparative Example 5 respectively show flocculation. When the cement slurry, drilling fluid and the spacer fluid system prepared in Example 2 are mixed, the thickening time of the slurry is extended. At 240°C, the thickening time of the mixed slurry is greater than 300min. It can be seen that the ultra-high temperature cementing spacer fluid system prepared in Example 2 has good chemical compatibility with drilling fluid and cement slurry. When the cement slurry, drilling fluid and the spacer fluid system prepared in Comparative Example 5 are mixed, the thickening time of the mixed slurry is greater than 300min at a temperature below 150°C, and it has good compatibility; at a temperature above 150°C, the thickening time of the mixed slurry is shortened to varying degrees; it can be seen that the anti-pollution ability of the spacer fluid system of Comparative Example 5 is weakened at high temperature and does not meet the construction requirements. This indicates that the anti-pollution agent of the present invention is compounded with two components, which plays a key role in promoting the three-phase compatibility of cement slurry, drilling fluid and spacer fluid in an environment above 150°C.
Claims
1. An ultra-high temperature cementing spacer fluid system, comprising the following components, in parts by weight: 100 parts of water, 1-6 parts of a suspension stabilizer, 3-10 parts of a flushing agent, 1-20 parts of an anti-pollution agent, 0.2-0.5 parts of a defoaming agent, and 90-400 parts of a weighting agent; in, The suspension stabilizer includes a polymer prepared from 2-acrylamide-2-methylpropane sulfonic acid, N-vinyl caprolactam, 1-vinylimidazole and octadecyl dimethyl allyl ammonium chloride as monomers; and the weight ratio of 2-acrylamide-2-methylpropane sulfonic acid, N-vinyl caprolactam, 1-vinylimidazole and octadecyl dimethyl allyl ammonium chloride is (15-25):(15-25):(7-15):(10-15).
2. The ultra-high temperature cementing spacer fluid system according to claim 1, wherein: The ultra-high temperature cementing isolation fluid system includes the following components in parts by weight: 100 parts of water, 2-5 parts of suspension stabilizer, 3-10 parts of flushing agent, 3-10 parts of anti-pollution agent, 0.2-0.5 parts of defoaming agent and 90-400 parts of weighting agent.
3. The ultra-high temperature cementing spacer fluid system according to claim 1 or 2, wherein: The suspension stabilizer is prepared by at least the following steps: dissolving 2-acrylamide-2-methylpropanesulfonic acid, N-vinyl caprolactam, 1-vinylimidazole, and octadecyldimethylallyl ammonium chloride in a weight ratio of (15-25):(15-25):(7-15):(10-15) in an appropriate amount of water to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 6.5-7.5 to obtain a second mixed solution; and then adding an initiator to the second mixed solution to carry out a polymerization reaction. After the reaction is completed, a polymer solution is obtained, which is the suspension stabilizer.
4. The ultra-high temperature cementing spacer fluid system according to claim 3, wherein: The weight ratio of 2-acrylamide-2-methylpropanesulfonic acid, N-vinylcaprolactam, 1-vinylimidazole, octadecyldimethylallylammonium chloride and water is (15-25):(15-25):(7-15):(10-15):(200-350).
5. The ultra-high temperature cementing spacer fluid system according to claim 3, wherein: Sodium hydroxide is used to adjust the pH value of the first mixed solution to 6.5-7.
5.
6. The ultra-high temperature cementing spacer fluid system according to claim 3, wherein: The initiator includes ammonium persulfate and sodium bisulfite; Preferably, based on 100% of the total weight of the second mixed solution, the amount of ammonium persulfate added is 0.4-0.8%, and the amount of sodium bisulfite added is 0.1-0.3%.
7. The ultra-high temperature cementing spacer fluid system according to claim 3, wherein: The polymerization reaction temperature is 50-70° C. and the reaction time is 2-5 hours.
8. The ultra-high temperature cementing spacer fluid system according to claim 1 or 2, wherein: The flushing agent comprises a mixture of a surfactant, an organic solvent and a chelating agent in a weight ratio of (20-35):(50-70):(10-15); Preferably, the surfactant includes one or a combination of lauryl glucoside, fatty alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether and sodium dodecylbenzene sulfonate; Preferably, the organic solvent comprises n-butanol; Preferably, the chelating agent comprises disodium EDTA and / or tetrasodium EDTA.
9. The ultra-high temperature cementing spacer fluid system according to claim 1 or 2, wherein: The anti-pollution agent comprises a mixture of a first anti-pollution agent and a second anti-pollution agent in a weight ratio of (40-80):(5-30), wherein the first anti-pollution agent comprises one or a combination of ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, polyaminopolyether methylenephosphonic acid, aminotrimethylenephosphonic acid and hydrolyzed polymaleic anhydride, and the second anti-pollution agent comprises sodium gluconate and / or sodium tripolyphosphate; Preferably, the first anti-pollution agent is selected from one or two of ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, polyaminopolyether methylenephosphonic acid, aminotrimethylenephosphonic acid and hydrolyzed polymaleic anhydride, and the second anti-pollution agent is selected from one of sodium gluconate and sodium tripolyphosphate.
10. The ultra-high temperature cementing spacer fluid system according to claim 1 or 2, wherein: The defoaming agent comprises one or a combination of tributyl phosphate, polyoxypropylene glycerol ether and polydimethylsiloxane.
11. The ultra-high temperature cementing spacer fluid system according to claim 1 or 2, wherein: The weighting agent includes one or a combination of barite powder, hematite powder and iron ore powder.
12. A method for preparing the ultra-high temperature cementing spacer fluid system according to any one of claims 1 to 11, comprising the following steps: 1-6 parts by weight of a suspension stabilizer is added to 100 parts by weight of water and stirred for a period of time; then 90-400 parts by weight of a weighting agent, 3-10 parts by weight of a flushing agent, and 1-20 parts by weight of an anti-pollution agent are added and stirred for a period of time; then 0.2-0.5 parts by weight of a defoaming agent is added to obtain the ultra-high temperature cementing isolation fluid system.
13. The preparation method according to claim 12, wherein: After adding the suspension stabilizer into the water, the stirring speed is 2000r / min±500r / min; Preferably, the suspension stabilizer is added to water and stirred for 1-5 minutes.
14. The preparation method according to claim 12, wherein: After adding weighting agent, flushing agent and anti-pollution agent, the stirring speed is 2000r / min±500r / min; Preferably, the stirring time after adding the weighting agent, flushing agent and anti-pollution agent is 2-10 minutes.
15. Use of the ultra-high temperature cementing spacer fluid system according to any one of claims 1 to 11 in cementing operations of special wells.
16. The use according to claim 15, wherein: The special wells include high-temperature and high-pressure gas wells, unconventional oil and gas wells, gas storage wells, deep wells, and ultra-deep wells.
17. The use according to claim 15, wherein: The bottom hole circulation temperature of the special well is below 240°C.
Citation Information
Cited By
Low-molecular-weight composite anti-pollution agent for well cementation
CN119875594A
Ultrahigh-temperature-resistant spacer fluid system as well as preparation method and application thereof
CN122127961A
Broad-spectrum anti-pollution spacer fluid for ultra-deep well cementation and preparation method of broad-spectrum anti-pollution spacer fluid
CN122302849A