Preparation method of high-fluorescence cellulose-based carbon quantum dots

By enzymatic pretreatment of natural cellulose and high-temperature hydrothermal method to prepare cellulose-based carbon quantum dots, the problem of insufficient fluorescence performance of cellulose-based CQDs was solved, and the effect of significantly improving fluorescence performance was achieved.

CN119039983AActive Publication Date: 2024-11-29GUANGXI UNIV

Patent Information

Application Number
CN202411149162.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing cellulose-based carbon quantum dots (CQDs) have insufficient fluorescence performance and are difficult to meet application needs. The existing research mainly relies on doping elements to regulate fluorescence performance, but there is a lack of research on pretreatment of natural cellulose.

Method used

By enzymatic pretreatment of natural cellulose, the enzyme solution product was obtained as a carbon source. The high-temperature hydrothermal method was used to react in a polytetrafluoroethylene lined reactor, dialysis and lyophilization were performed to prepare highly fluorescent cellulose-based carbon Quantum dots.

Benefits of technology

The fluorescence performance of CQDs was improved, and the significant impact of the enzymatic decomposition process on the fluorescence performance was proved. The method of using enzymatic decomposition as a carbon source is highly operable, and the fluorescence intensity and quantum yield were significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039983A_ABST
    Figure CN119039983A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of high-fluorescence cellulose-based carbon quantum dots. The method comprises the steps of enzymolysis of cellulose, acquisition of a carbon source and preparation of CQDs. The CQDs are prepared after the natural cellulose is subjected to enzymolysis pretreatment, so that the purpose of improving the fluorescence property of the CQDs is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the technical field of composite materials, and in particular to a method for preparing high-fluorescence cellulose-based carbon quantum dots. [Background technology]

[0002] Cellulose is one of the most abundant renewable organic resources on earth and is widely present in plant cell walls. However, due to its strong mechanical structure and high chemical stability, cellulose is difficult to be used directly. By enzymatically degrading cellulose into monosaccharides or oligosaccharides such as glucose, cellulose can be used as a resource and its economic value can be improved. Among the products of cellulose enzymatic hydrolysis, glucose has become a high-quality raw material for the preparation of CQDs because of its simple structure and easy process control.

[0003] The common problem encountered by cellulose-based CQDs at present is that they cannot meet the expected fluorescence performance requirements. A common solution is to dope heteroatoms, such as amines and alkali metals as reactive ligands. Some researchers believe that nitrogen (N) doping will enter the carbon core formation process and participate in the formation of graphene-like structures. In addition, N-doped cellulose-based CQDs have excellent fluorescence stability and are more sensitive to Fe 3+ The selective sensitivity of the dopant confirms the effectiveness of the dopant. In recent years, researchers have proposed a new method for synthesizing CQDs with dual element doping. Cellulose extracted from sawdust can be co-doped with Mg(OH)2 and ethylenediamine to produce strong green fluorescent cellulose-based CQDs. Jiang Fan et al. used microcrystalline cellulose as a carbon source and polyethyleneimine as a nitrogen source to prepare high fluorescence quantum yield CQDs by hydrothermal method in a certain proportion, and the CQDs were sensitive to Fe 3+ Huang Hailong et al. used cellulose hydrogel as a precursor to prepare CQDs of different particle sizes, which can be used to detect heavy metal ions Hg 2+ Hu Donghao et al. prepared a novel nanofiber that can simultaneously detect Fe by microwave-assisted synthesis using 2,2,6,6-tetramethylpiperidin-1-oxyl free radical-mediated oxidized cellulose nanofibers and 4,7,10-trioxa-1,13-tridecanediamine as precursors. 3+ and Mn 2+ Fluorescent carbon dots.

[0004] At present, most of the existing research on the regulation of the fluorescence properties of C-CQDs is still based on doping with impurities, starting from the carbon precursor cellulose, and preparing CQDs by pre-treating the natural cellulose to improve its fluorescence properties. However, there is almost no research found so far. [Summary of the invention]

[0005] In view of the above, it is necessary to provide a method for preparing highly fluorescent cellulose-based carbon quantum dots, by preparing CQDs after pretreatment of natural cellulose such as enzymatic hydrolysis, so as to achieve the purpose of improving its fluorescence performance.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing highly fluorescent cellulose-based carbon quantum dots, the method comprising the following steps:

[0008] (1) Enzymatic hydrolysis of cellulose: Cellulose and cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 4.5-5.0 with sodium citrate buffer, followed by enzymatic hydrolysis;

[0009] (2) Obtaining a carbon source: inactivating the cellulase in the reaction system of step (1) at high temperature, and obtaining an enzymatic hydrolysis product as a carbon source for later use;

[0010] (3) Preparation of CQDs: The carbon source obtained in step (2) is added to a polytetrafluoroethylene-lined reactor, and then the reactor is placed in an environment of 180-220°C for reaction for 10-15 hours, and naturally cooled to room temperature. The product in the reactor is filtered, and the supernatant is collected, dialyzed, concentrated, and freeze-dried to obtain a solid CQDs product.

[0011] Furthermore, the cellulose concentration in step (1) is 1.5-2.5% w / v, and the cellulase activity is 10-20 FPU / g.

[0012] Furthermore, in step (1), the enzymatic hydrolysis temperature is 45-55° C., and the enzymatic hydrolysis time is 5-40 min.

[0013] Furthermore, the molecular cutoff of the dialysis bag in step (3) is 1000Da.

[0014] Furthermore, the carbon source can be obtained by: inactivating the cellulase in the reaction system of step (1) at high temperature, then washing, filtering and drying the solid product after cellulolysis in deionized water, and then mixing the carbon source with deionized water in a ratio of adding 25 ml of deionized water to 1 g of the dry product to obtain the carbon source.

[0015] The present invention has at least the following beneficial effects:

[0016] In the present application, the enzymatic hydrolysis product obtained by enzymatic hydrolysis of cellulose by cellulase is used as a carbon source to prepare CQDs. Experiments have shown that the CQDs obtained by the method of the present application have high fluorescence properties, which proves the interaction between cellulose and its enzymatic hydrolysis solution during the formation of CQDs. Enzymatic hydrolysis is feasible for improving the fluorescence properties of CQDs.

Brief Description of the Drawings

[0017] Figure 1 Schematic diagram of the formation process of cellulose-based CQDs. [Specific implementation method]

[0018] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0019] Embodiment 1:

[0020] This embodiment is a method for preparing highly fluorescent cellulose-based carbon quantum dots, the method comprising the following steps:

[0021] (1) Enzymatic hydrolysis of cellulose: 1.5% w / v cellulose and 10 FPU / g cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 4.5 with sodium citrate buffer, followed by enzymatic hydrolysis at 45°C for 5 min at a rotation speed of 150 rpm;

[0022] (2) Obtaining a carbon source: inactivating the cellulase in the reaction system of step (1) at high temperature, and obtaining an enzymatic hydrolysis product as a carbon source for later use;

[0023] (3) Preparation of CQDs: The carbon source obtained in step (2) was added to a 50 ml polytetrafluoroethylene-lined reactor, and the reactor was placed in an environment of 180°C for reaction for 10 h, and naturally cooled to room temperature. The product in the reactor was filtered, and the supernatant was collected and dialyzed with a molecular retention capacity of 1000 Da, concentrated, and freeze-dried to obtain a solid CQDs product.

[0024] Embodiment 2:

[0025] This embodiment is a method for preparing highly fluorescent cellulose-based carbon quantum dots, the method comprising the following steps:

[0026] (1) Enzymatic hydrolysis of cellulose: 2.0% w / v cellulose and 15 FPU / g cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 4.8 with sodium citrate buffer, followed by enzymatic hydrolysis at 50°C for 40 min at a rotation speed of 150 rpm;

[0027] (2) Obtaining a carbon source: inactivating the cellulase in the reaction system of step (1) at high temperature, and obtaining an enzymatic hydrolysis product as a carbon source for later use;

[0028] (3) Preparation of CQDs: The carbon source obtained in step (2) was added to a 50 ml polytetrafluoroethylene-lined reactor, and the reactor was placed in an environment of 200°C for reaction for 12 h, and naturally cooled to room temperature. The product in the reactor was filtered, and the supernatant was collected and dialyzed to a molecular cutoff of 1000 Da, concentrated, and freeze-dried to obtain a solid CQDs product.

[0029] Embodiment 3:

[0030] This embodiment is a method for preparing highly fluorescent cellulose-based carbon quantum dots, the method comprising the following steps:

[0031] (1) Enzymatic hydrolysis of cellulose: 2.5% w / v cellulose and 20 FPU / g cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 5.0 with sodium citrate buffer, followed by enzymatic hydrolysis at 55°C for 40 min at a rotation speed of 150 rpm;

[0032] (2) Obtaining a carbon source: inactivating the cellulase in the reaction system of step (1) at high temperature, and obtaining an enzymatic hydrolysis product as a carbon source for later use;

[0033] (3) Preparation of CQDs: The carbon source obtained in step (2) was added to a 50 ml polytetrafluoroethylene-lined reactor, and then the reactor was placed in an environment of 220°C for reaction for 15 h, and naturally cooled to room temperature. The product in the reactor was filtered, and the supernatant was collected and dialyzed with a molecular retention capacity of 1000 Da, concentrated, and freeze-dried to obtain a solid CQDs product.

[0034] Embodiment 4:

[0035] This embodiment is a method for preparing highly fluorescent cellulose-based carbon quantum dots, the method comprising the following steps:

[0036] (1) Enzymatic hydrolysis of cellulose: 2.0% w / v cellulose and 15 FPU / g cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 4.8 with sodium citrate buffer, followed by enzymatic hydrolysis at 50°C for 40 min at a rotation speed of 150 rpm;

[0037] (2) Obtaining a carbon source: The cellulase in the reaction system of step (1) is inactivated at high temperature, and then the solid product after the cellulolysis is washed, filtered, and dried in deionized water. Then, 0.5 g of the obtained dry product is mixed with 25 ml of deionized water to obtain a carbon source for use;

[0038] (3) Preparation of CQDs: The carbon source obtained in step (2) was placed in a 50 ml polytetrafluoroethylene-lined reactor, and the reactor was then placed in an environment of 200°C for reaction for 12 h, and naturally cooled to room temperature. The product in the reactor was filtered, and the supernatant was collected and dialyzed with a molecular retention capacity of 1000 Da, concentrated, and freeze-dried to obtain a solid CQDs product.

[0039] Test example:

[0040] A 200 mL reaction system was set in a 500 mL conical flask, 2% (w / v) cellulose and 15 FPU / g cellulase were added, and the enzymolysis time was controlled to be 0 min, 1 min, 5 min, and 40 min, respectively, to obtain products with different polymerization degrees. Except for the different enzymolysis time, the other methods were respectively according to the method described in Example 2 and the method described in Example 4, and the difference between the two was only the different methods of obtaining the carbon source;

[0041] Cellulose with the above eight polymerization degrees of cellulose was used as the carbon source, and cellulose-based carbon quantum dots were prepared by hydrothermal method; wherein, in Example 4, the enzymatic hydrolysis time of 0min, 1min, 5min, and 40min corresponded to C-CQDs0, C-CQDs1, C-CQDs5, C-CQDs 40 In Example 2, the enzymatic hydrolysis time was 1 min, 5 min, and 40 min, respectively corresponding to E-CQDs1, E-CQDs5, and E-CQDs 40 ;

[0042] The physicochemical properties and optical properties of C-CQDs and E-CQDs were characterized, and the relationship between the physicochemical properties and optical properties of C-CQDs and E-CQDs and the degree of polymerization of cellulose was explored.

[0043] Characterization:

[0044] The degree of polymerization of cellulose after enzymatic hydrolysis was determined by the copper ethylenediamine method using an Ubbelohde viscometer. The glucose content in the system was measured by high performance liquid chromatography (HPLC) to measure the degree of hydrolysis at the corresponding stage. Cellulose powder samples and CQDs powder samples before and after enzymatic hydrolysis were tested using an X-ray diffractometer (Rigaku D / MAX 2500V, Japan).

[0045] The scanning range is 2θ=5°-80°. The UV-Vis absorption spectrum of the CQDs solution was measured in the range of 200-800 nm using an ultraviolet visible spectrophotometer (UV-Vis, Hitachi U-4100UV-Vis, Japan).

[0046] Fourier transform infrared spectrometer (FTIR, TENSOR II, Bruker, Germany) was used to determine the chemical structure of CQDs in attenuated total reflection (ATR) mode. X-ray photoelectron spectroscopy (XPS, Thermo Fisher Scientific K-alpha+, USA) was used to determine the content of elements such as carbon and oxygen and the composition of functional groups on the surface of CQDs. A transmission electron microscope (TEM, FEI TECNAI G2 F30, USA) was used to observe the microstructure of CQDs. A micro-Raman spectrometer (Raman) was used to analyze the degree of graphitization of CQDs. The laser wavelength of the instrument was 630nm and the power was 0.10mW. A fluorescence spectrometer (Hitachi RF-5301PC, Japan) was used to measure the fluorescence spectrum (FLs) and quantum yield of CQDs. When measuring FLs, the width of the excitation slit and the emission slit were both 3nm. Through the above characterization, the formation mechanism of cellulose-based CQDs can be inferred, such as Figure 1 shown.

[0047] result:

[0048] The fluorescence intensity and fluorescence quantum yield at each enzymatic hydrolysis time were tested, and the data were recorded as shown in Table 1:

[0049] Table 1

[0050] Fluorescence intensity Fluorescence quantum yield (%) <![CDATA[C-CQDs0]]> 56539 0.7% <![CDATA[C-CQDs1]]> 67375 0.71% <![CDATA[C-CQDs5]]> 93000 0.99% <![CDATA[C-CQDs 40 ]]> 103314 1.87% <![CDATA[E-CQDs1]]> 117628 1.98% <![CDATA[E-CQDs5]]> 127373 2.51% <![CDATA[E-CQDs 40 ]]> 143497 2.77%

[0051] According to the data in Table 1, it is proved that the preparation of CQDs using enzymatic cellulose as a carbon precursor can improve the fluorescence performance of CQDs. In addition, the test results also found that the fluorescence intensity and fluorescence quantum yield of using the enzymatic hydrolysis product directly as a carbon source (E-CQDs) are higher than the method of washing the enzymatic hydrolysis product with deionized water, drying it, and then mixing it with deionized water as a carbon source (C-CQDs).

[0052] The above examples only express several embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing highly fluorescent cellulose-based carbon quantum dots, characterized in that: The method comprises the following steps: (1) Enzymatic hydrolysis of cellulose: Cellulose and cellulase were placed in a conical flask, and the pH value of the reaction system was maintained at 4.5-5.0 with sodium citrate buffer, followed by enzymatic hydrolysis; (2) Obtaining a carbon source: inactivating the cellulase in the reaction system of step (1) at high temperature, and obtaining an enzymatic hydrolysis product as a carbon source for later use; (3) Preparation of CQDs: The carbon source obtained in step (2) is added to a polytetrafluoroethylene-lined reactor, and then the reactor is placed in an environment of 180-220°C for reaction for 10-15 hours, and naturally cooled to room temperature. The product in the reactor is filtered, and the supernatant is collected, dialyzed, concentrated, and freeze-dried to obtain a solid CQDs product.

2. The method according to claim 1, characterized in that The cellulose concentration in step (1) is 1.5-2.5% w / v, and the cellulase activity is 10-20 FPU / g.

3. The method according to claim 1, characterized in that The enzymatic hydrolysis temperature in step (1) is 45-55° C., and the enzymatic hydrolysis time is 1-40 min.

4. The method according to claim 1, characterized in that: The molecular cutoff of the dialysis bag in step (3) is 1000Da.

Citation Information

Patent Citations

  • Method for preparing water-soluble yellow fluorescent carbon quantum dot by taking bagasse as raw material

    CN106634981A

  • Method for preparing water-soluble carbon quantum dots from sisal hemp as raw material

    CN106753354A

  • Method for detecting Fe(III) ions by using nitrogen-doped biomass-based carbon quantum dots

    CN109880619A

  • Acidic carbon quantum dot, preparation method and application thereof

    CN111892038A

  • Primers for RT-LAMP based detection of Newcastle disease virus and its use

    KR1020240066478A

Cited By

  • Artemisia argyi-based nitrogen-sulfur co-doped carbon quantum dot as well as preparation method and application thereof

    CN122060488A