Carbon-oxygen balance adjusting composition for hard alloy and application of carbon-oxygen balance adjusting composition

By using metal oxides and molding agents to achieve carbon-oxygen equilibrium in cemented carbide recovery technology, the carbon-oxygen equilibrium problem in cemented carbide is solved, product quality and production efficiency are improved, and cost and time are reduced.

CN119040682APending Publication Date: 2024-11-29ZHENGTONG SPECIAL MATERIAL FACTORY HI & NEW TECH ZONE CHENGDU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411150838.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

It is difficult to achieve carbon-oxygen balance in existing cemented carbide recycling technologies, resulting in unstable product quality, and traditional carbon control methods have problems such as quality defects, high cost and long time.

Method used

Carbon-oxygen balance adjustment composition for cemented carbide, including metal oxides as decarbonization agents and molding agents as deoxidants, to achieve carbon-oxygen balance by adjusting its reasonable matching amount, solve the carburization and decarbonization problems, and use magnetism Saturation measurement accurately controls carbon.

Benefits of technology

It effectively solves the problems of carburizing and decarbonization, improves the accuracy of product quality control, reduces costs and time, improves production efficiency, and makes up for the shortcomings of the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003615950000111
    Figure BDA0005003615950000111
  • Figure BDA0005003615950000112
    Figure BDA0005003615950000112
  • Figure BDA0005003615950000121
    Figure BDA0005003615950000121
Patent Text Reader

Abstract

The invention relates to a carbon-oxygen balance adjusting composition for hard alloy and application thereof, and relates to hard alloy, in particular to the technical field of hard alloy recovery, the carbon-oxygen balance adjusting composition for hard alloy comprises a decarburizing agent and a deoxidizing agent; the decarburizing agent is a metal oxide; the deoxidizing agent is a forming agent. On one hand, the metal oxide is used as the decarburizing agent, so that the problems of carburization and removal of C in a forming agent can be more effectively solved, the consumption is low, the cost is low, and the time is saved. And on the other hand, the forming agent serves as a deoxidizing agent, deoxidization is achieved, and the problem of C deficiency in the alloy can be solved through residual carbon in the forming agent. Carbon-oxygen balance is achieved by adjusting the reasonable matching amount of the metal oxide and the forming agent. The problems of carburization and decarburization can be solved, and the universal effect is achieved. And the problem of accurate carbon control can be solved by magnetic saturation measurement. And obviously, the method has higher control accuracy on the alloy quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to cemented carbide, in particular to the technical field of recycling cemented carbide, and more particularly to a carbon-oxygen balance regulating composition for cemented carbide and application thereof. Background Art

[0002] As an indispensable and important material in modern industry, cemented carbide is widely used in machinery manufacturing, geological mining, construction, electronics and chemical industry. It is mainly composed of metal elements such as tungsten carbide (WC) and cobalt (Co), and is favored for its high hardness, high strength and high wear resistance. However, with the development of industry, the consumption of cemented carbide has increased sharply, and the problem of recycling and reuse of waste cemented carbide has become increasingly prominent. Waste cemented carbide contains a large amount of tungsten (W) and cobalt (Co). As rare metals, the ore reserves of these elements are limited and the difficulty of mining is gradually increasing. Therefore, the recycling and reuse of tungsten and cobalt elements in waste cemented carbide not only has significant economic benefits, but also has important significance for saving resources and developing a circular economy.

[0003] Early methods for recycling scrap cemented carbide mainly include saltpeter smelting, zinc melting, sodium sulfate smelting and phosphoric acid leaching, but these methods have problems such as high energy consumption, low purity of recycled alloy powder, complex operation and potential harm to the environment and workers' health. With the advancement of technology, emerging methods such as electrochemical dissolution (electrodissolution or electrolysis), mechanical crushing, oxidation and so on have gradually emerged, and have improved the recycling efficiency and product quality to a certain extent. However, these existing methods still face many challenges. Among them, in the production and recycling process of cemented carbide, achieving carbon-oxygen balance and accurately controlling the carbon content are key factors to ensure product quality. This not only affects the microstructure of the alloy, but is also directly related to the mechanical properties and service life of the alloy.

[0004] Therefore, achieving carbon-oxygen balance and precise carbon control are major quality issues related to cemented carbide products. It is also a technical problem that has been difficult to solve for many years. In particular, large and special-shaped products often use rubber molding agents, which are more difficult to solve carbon-oxygen balance and precise carbon control problems than paraffin molding agents. If not solved well, product decarburization and carburization often occur, resulting in a large number of waste products. If the carbon control accuracy is not enough, the product cannot meet the requirements of high-quality products in the application field. Therefore, it is very important to solve the above problems in the production and recycling of cemented carbide. In order to obtain high-quality cemented carbide products, it is necessary to solve the internal carbon-oxygen balance of the alloy during the preparation process, and on this basis, accurately control carbon.

[0005] At present, the traditional carbon (C) control technology methods mainly include the following methods: 1. Use unsaturated C WC to adjust the excess carbon in alloy production. The raw material lacks C and "eats" the residual C of the molding agent. 2. Use saturated C WC and use W powder to adjust the excess C in alloy production. Add W powder and residual C in the molding agent to form an incomplete and irregular WC to adjust carburizing. 3. Use long-term low-temperature vacuum or hydrogen debonding sintering to remove the molding agent before the molding agent (CH compound) reaches C and H cracking (before there is residual C). The debonding time is 6.5-48 hours. 4. Use saturated C WC and use low-temperature paraffin as the molding agent. The molding agent does not produce residual C or a small amount of residual C. These methods focus on how to debond cemented carbide. Debonding can solve the problem of residual C in the molding agent. It can ensure that the cemented carbide product has a reasonable C content. The essence is to maintain a balance between C and oxygen content in alloy production. Too much C will lead to carburization of the product, too much oxygen will lead to less C, and the product will lose C. The balance means no loss of C and no C infiltration. The above methods have their own advantages and disadvantages. Method 1: Use unsaturated WC. WC has many quality defects, which seriously affect the quality. Method 2: Use W powder to adjust C. The amount of W powder used is large, the cost is high, and the false WC affects the quality (false WC refers to WC that is not generated according to the specifications). Method 3: The degumming time is too long, the electricity and labor costs are too high, and it is difficult to degumming completely. Method 4: Paraffin has poor adhesion, large amount is used, it is easy to flow, volatilize, and seriously pollute the furnace. Once degumming and C infiltration occur, the neutral molding agent paraffin cannot solve any problems. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a carbon-oxygen balance regulating composition for cemented carbide and application thereof.

[0007] In a first aspect, the present invention provides a carbon-oxygen balance regulating composition for cemented carbide, wherein the carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizer and a deoxidizer;

[0008] The decarburizing agent is a metal oxide;

[0009] The deoxidizer is a molding agent.

[0010] Furthermore, the metal oxide includes at least one of tungsten trioxide and titanium dioxide.

[0011] Furthermore, the molding agent includes a compression-molded rubber molding agent and a mixed molding agent for injection molding and extrusion molding; the compression-molded rubber molding agent includes at least one of organic rubber and polymer resin rubber, and the mixed molding agent for injection molding and extrusion molding includes at least one of paraffin, polyethylene, and a dispersant.

[0012] In a second aspect, the present invention provides a use of the carbon-oxygen balance regulating composition for cemented carbide as described in any one of the first aspects in controlling the carbon-oxygen balance of cemented carbide and recovering cemented carbide.

[0013] In a third aspect, the present invention provides a method for controlling the carbon-oxygen balance of cemented carbide, the method comprising using the carbon-oxygen balance regulating composition for cemented carbide according to any one of the first aspects to regulate the carbon-oxygen balance of cemented carbide, the method comprising the following steps:

[0014] Purchase saturated carbon tungsten carbide, including raw materials and recycled materials; perform carbon content analysis and calculation for WC with unknown carbon content, determine the carbon content in WC, and use it as a data reference for adding carbon-oxygen balance adjustment composition for cemented carbide;

[0015] Adding a preset proportion of decarburizing agent to the WC raw material to obtain a first mixed material;

[0016] Adding a preset proportion of deoxidizer to the first mixed material to obtain a second mixed material;

[0017] Pressing the second mixed material into a mold to obtain a test block;

[0018] The test block is debonded and sintered, and the sintered test block is tested for carburization and decarburization; if it is not decarbonized or carburized, it can be directly put into mass production. Specifically, 1. If the product is decarbonized and carburized after burning, it must be unqualified. For the decarbonization phenomenon, the amount of oxidant added can be reduced, and the amount of forming agent can be increased. The amount of binder in the forming agent cannot be >1.3%. If it is >1.3%, you should consider changing WC instead of using this method to solve it. If the product is carburized after burning, the amount of oxidant can be increased, and the amount of forming agent can be reduced. The oxidant cannot be >2% of the material. The reduction in the amount of forming agent cannot change the pressing and forming performance. If it still cannot be solved, this carbon-oxygen balance method should be abandoned. Instead, purchase WC with a suitable carbon content. 2. If the product is burned, it is neither decarbonized nor carburized. Use the magnetic saturation measurement method to further finely measure carbon and finely adjust the C amount on the basis of carbon-oxygen balance to achieve better quality on qualified products.

[0019] Furthermore, in terms of weight percentage, the total C content in the WC raw material is within the range of 6.13%±0.02.

[0020] Further, for saturated WC: 1) the amount of the decarburizer added is 0.2-1.0 wt% of the total amount of the mixture; 2) the amount of the binder added in the molding agent is 0.9-1.3 wt% of the mixture;

[0021] For unsaturated C WC: 1) the amount of oxidant added is determined according to the C saturation degree of WC; 2) the amount of binder added in the molding agent is 0.9-1.3wt% of the mixture.

[0022] Furthermore, the relative magnetic saturation values ​​of the non-decarburized and carburized test blocks are calculated, and the amount of the selected decarburizer and deoxidizer is determined by comparing the brand and other performance test values; then, the carbon-oxygen balance of the cemented carbide is batch-controlled based on the obtained amount of decarburizer and deoxidizer, and then mass production is started after the control.

[0023] In a fourth aspect, the present invention provides a method for recovering cemented carbide, the method comprising recovering cemented carbide using the carbon-oxygen balance regulating composition for cemented carbide according to any one of the first aspects, the method comprising the following steps:

[0024] Determining the C content in WC in the scrap alloy material, and judging whether the scrap alloy material is saturated with C, lacking in C, or oversaturated with C;

[0025] Adding a decarburizing agent in a preset proportion to the waste alloy material lacking in carbon or being oversaturated in carbon to obtain a third mixed material;

[0026] Adding a preset proportion of a deoxidizer to the third mixed material to obtain a fourth mixed material;

[0027] Pressing and molding the fourth mixed material to obtain a test block;

[0028] The test block is debonded and sintered to detect whether the sintered test block is carburized or decarburized; if it is not decarburized or carburized, it can directly enter mass production.

[0029] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:

[0030] The embodiment of the present invention provides a carbon-oxygen balance regulating composition for cemented carbide. On the one hand, the present invention uses metal oxide as a decarburizing agent, which can more effectively solve the problems of carburization and C in the molding agent, and the dosage is small, the cost is low, and time is saved. On the other hand, the present invention uses a molding agent as a deoxidizer, which not only achieves deoxidation, but also the residual carbon in the molding agent can solve the problem of C deficiency in the alloy. The present invention achieves carbon-oxygen balance by adjusting the reasonable matching amount of metal oxide and molding agent. It can solve both carburization and decarburization problems, and has a universal effect. Magnetic saturation measurement can also be used to solve the problem of precise carbon control. Obviously, it has a higher control accuracy on the quality of the alloy, which makes up for the shortcomings of the prior art. Specifically:

[0031] 1. Any component in the metal oxide is an oxidant, which can remove the carbon in the molding agent and the carbon in the product. For example, WO3 and TiO2 are used. In addition to O, metals are also carbon removers. The oxygen in the metal oxide can react with the carbon in the alloy (or the residual carbon in the rubber) to generate CO and CO2. Metals and carbon can also generate metal carbides. Such as WC and TiC. It can more effectively solve the problem of carburization and carbon in the molding agent.

[0032] 2. Residual carbon in the forming agent can solve the problem of carbon deficiency in the alloy. The lack of carbon in the alloy will cause the product to lose carbon. Adjusting the amount of the forming agent can solve this defect.

[0033] 3. Using metal oxide as the carbon adjuster of alloy, the dosage is small and the cost is low. According to our test, if 20g of W powder is used, only 4g of TiO2 is needed, which reduces the dosage by 80% and the cost by 90%.

[0034] 4. Using metal oxide to remove carbon can greatly save time. The traditional degumming time is as long as 6.5 to 48 hours, and the vacuum degumming time of this method is only more than 5 hours. The production efficiency is greatly improved.

[0035] 5. Paraffin wax has poor adhesion and is suitable for making some simple and small products. For complex and large products, rubber molding agents are better. The pressed finished products have high density, quality and strength.

[0036] The melting point and sublimation point of paraffin wax are low, and the dosage is about twice that of rubber molding agent. It is easy to stick to the furnace and pipes. The pollution is serious and the cleaning labor cost is high. It is easy to maintain neutral balance when paraffin wax is used as molding agent, but the performance is single, and it cannot solve the problems of decarbonization and carburization generated by non-molding agent. It is difficult to achieve carbon-oxygen balance when needed.

[0037] 6. This method achieves carbon-oxygen balance by adjusting oxides and forming agents. It can solve both carburization and decarburization problems. It has a universal effect. It can also use magnetic saturation measurement to solve the problem of precise carbon control. Obviously, it has a higher control accuracy on the quality of the alloy.

[0038] 7. This method can pre-prepare different amounts of glue and metal oxides for trial firing before adding the molding agent. According to the trial firing results, one or two amounts can be selected and adjusted to coordinate the ratio, so as to eliminate the waste caused by decarburization and carburization. It greatly improves the product yield and reduces the loss cost.

[0039] 8. This product can use saturated WC. It breaks the tradition that rubber molding agents can only use unsaturated WC to produce cemented carbide. The application of saturated WC greatly improves the quality level of rubber molding agent cemented carbide products. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0042] In a first aspect, the present invention provides a carbon-oxygen balance regulating composition for cemented carbide, the carbon-oxygen balance regulating composition for cemented carbide comprising a decarburizer and a deoxidizer;

[0043] The decarburizing agent is a metal oxide;

[0044] The deoxidizer is a molding agent.

[0045] The embodiment of the present invention provides a carbon-oxygen balance regulating composition for cemented carbide. On the one hand, the present invention uses metal oxide as a decarburizing agent, which can more effectively solve the problems of carburization and C in the molding agent, and the dosage is small, the cost is low, and time is saved. On the other hand, the present invention uses a molding agent as a deoxidizer, which not only achieves deoxidation, but also the residual carbon in the molding agent can solve the problem of C deficiency in the alloy. The present invention achieves carbon-oxygen balance by adjusting the reasonable matching amount of metal oxide and molding agent. It can solve both carburization and decarburization problems, and has a universal effect. Magnetic saturation measurement can also be used to solve the problem of precise carbon control. Obviously, it has a higher control accuracy on the quality of the alloy, which makes up for the shortcomings of the prior art. Specifically:

[0046] 1. Any component in the metal oxide is an oxidant, which can remove the carbon in the molding agent and the carbon in the product. For example, WO3 and TiO2 are used. In addition to O, metals are also carbon removers. The oxygen in the metal oxide can react with the carbon in the alloy (or the residual carbon in the rubber) to generate CO and CO2. Metals and carbon can also generate metal carbides. Such as WC and TiC. It can more effectively solve the problem of carburization and carbon in the molding agent.

[0047] 2. Residual carbon in the forming agent can solve the problem of carbon deficiency in the alloy. The lack of carbon in the alloy will cause the product to lose carbon. Adjusting the amount of the forming agent can solve this defect.

[0048] 3. Using metal oxide as the carbon adjuster of alloy, the dosage is small and the cost is low. According to our test, if 20g of W powder is used, only 4g of TiO2 is needed, which reduces the dosage by 80% and the cost by 90%.

[0049] 4. Using metal oxide to remove carbon can greatly save time. The traditional degumming time is as long as 6.5 to 48 hours, and the vacuum degumming time of this method is only more than 5 hours. The production efficiency is greatly improved.

[0050] 5. Paraffin wax has poor adhesion and is suitable for making some simple and small products. For complex and large products, rubber molding agents are better. The pressed finished products have high density, quality and strength.

[0051] The melting point and sublimation point of paraffin wax are low, and the dosage is about twice that of rubber molding agent. It is easy to stick to the furnace and pipes. The pollution is serious and the cleaning labor cost is high. It is easy to maintain neutral balance when paraffin wax is used as molding agent, but the performance is single, and it cannot solve the problems of decarbonization and carburization generated by non-molding agent. It is difficult to achieve carbon-oxygen balance when needed.

[0052] 6. This method achieves carbon-oxygen balance by adjusting oxides and forming agents. It can solve both carburization and decarburization problems. It has a universal effect. It can also use magnetic saturation measurement to solve the problem of precise carbon control. Obviously, it has a higher control accuracy on the quality of the alloy.

[0053] 7. This method can pre-prepare different amounts of glue and metal oxides for trial firing before adding the molding agent. According to the trial firing results, one or two amounts can be selected and adjusted to coordinate the ratio, so as to eliminate the waste caused by decarburization and carburization. It greatly improves the product yield and reduces the loss cost.

[0054] 8. This product can use saturated WC. It breaks the tradition that rubber molding agents can only use unsaturated WC to produce cemented carbide. The application of saturated WC greatly improves the quality level of rubber molding agent cemented carbide products.

[0055] In some specific embodiments, the metal oxide includes at least one of tungsten trioxide and titanium dioxide.

[0056] In some specific embodiments, the molding agent includes a compression-molded rubber molding agent and a mixed molding agent for injection molding and extrusion molding; the compression-molded rubber molding agent includes at least one of organic rubber and polymer resin rubber, such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), chloroprene rubber (CR), butadiene rubber (BR), etc.; the mixed molding agent for injection molding and extrusion molding includes at least one of paraffin, polyethylene, and a dispersant.

[0057] In some specific embodiments, the application of the carbon-oxygen balance regulating composition for cemented carbide may include the following process:

[0058] 1. When purchasing cemented carbide raw materials (whether virgin or recycled), strictly control that WC must be saturated carbon. The carbon content is generally required to be within 6.13% ± 0.03. The oxygen content of its main components: virgin materials < 0.05%, recycled materials ≤ 0.5%. Free carbon < 0.03%. Process technicians must strictly control the carbon and oxygen indicators of the feed, classify and file, and track and manage the carbon and oxygen balance of production and user use.

[0059] Second, use two balancers to adjust the carbon-oxygen balance of cemented carbide to achieve no decarburization and no carburization. Decarburizer: use metal oxides, the best of which are WO3 (tungsten trioxide) and titanium dioxide. Deoxidizer: use molding agents, including rubber molding agents for compression molding, and mixed molding agents for injection molding and extrusion molding.

[0060] Third, on the basis of the above two, the amount of binder mixed with the molding agent is selected between 0.9 and 1.3% to ensure the strength and quality of the pressed products of different products. The residual carbon content of the molding agent during sintering is adjusted with a metal oxidant. The general reaction formula is: NOn+nC=N+nCO (N represents metal, O represents oxygen, C represents carbon, and n represents the amount of C and O). Under the action of metal oxides, the carbon of the product is oxidized or the metal is carburized (NC), and the product reaches neutrality. There is neither decarburization nor carburization. That is, the crystal phase structure C of the cemented carbide product is between Coo-CO2, and individual fine grains are within CO4.

[0061] Fourth, based on the above two and three, the amount of molding agent and binder is accurately adjusted, such as 1.0, 1.05, 1.08, 1.10...1.30, and the specific position of the carbon content of the product between 81% and 93% is determined by relative magnetic saturation. By comparing the product working condition application effect, the optimal effect position of the product carbon content is determined. Achieve precise control of the product C and provide the most optimized product.

[0062] The magnetic saturation value of the alloy can be measured by a magnetic saturation meter. The relative magnetic saturation (%) can be calculated; the corresponding grade can be checked from the table: 90% C value, compared with the measured value. The relative magnetic saturation of the product can be determined, and the application effect can be referred to to determine the optimal C value of the alloy, so as to achieve accurate control of the C value of the product.

[0063] For example:

[0064] The implementation method includes the following process:

[0065] 1. Take 5-6 portions of 100g of mixed material (fully recycled material, recycled WC + cobalt (nickel)) before adding glue, add 0.7g Ti02, and add 5, 6, 7, 8, 9, 10g of forming agent respectively. Press the test block, heat it from 0 to 600 degrees in a vacuum furnace, and debond it for 5.30 hours according to the debonding process. Then sinter it to 1450 degrees according to normal products. Cool and check the metallographic structure of the test block after it is taken out of the furnace. If the amount of glue added is decarbonized (such as 5g) or carburized (such as 9g, 10g), it is not considered. If there is no decarbonization and carburization, such as 6g, 7g, 8g. Send it for magnetic saturation detection, and calculate the relative magnetic saturation and the corresponding grade C in the two-phase area in the figure, which is close, such as yG6, YG8, and yG10. The corresponding C content is similar. If the amount of glue added is 6g, the oxidant used for the large amount of glue added is T102, 0.7%, and the glue amount is 6%. The C and 02 balance can be achieved (no C loss, no C penetration), and the C amount can be more accurately measured under the guidance of relative magnetic saturation measurement, ensuring high output quality.

[0066] 2. Based on the above 1, change Ti02 from 0.7% to 0.4%, and keep other factors unchanged to achieve C, 0 balance. Accurately control C.

[0067] In a second aspect, based on the same inventive concept, the present invention provides the use of the carbon-oxygen balance regulating composition for cemented carbide described in any one of the first aspects in controlling the carbon-oxygen balance of cemented carbide and recovering cemented carbide.

[0068] In a third aspect, based on the same inventive concept, the present invention provides a method for controlling the carbon-oxygen balance of cemented carbide, the method comprising using the carbon-oxygen balance regulating composition for cemented carbide according to any one of the first aspects to regulate the carbon-oxygen balance of cemented carbide, the method comprising the following steps:

[0069] Purchase saturated carbon tungsten carbide, including raw materials and recycled materials; perform carbon content analysis and calculation for WC with unknown carbon content, determine the carbon content in WC, and use it as a data reference for adding carbon-oxygen balance adjustment composition for cemented carbide;

[0070] Adding a preset proportion of decarburizing agent to the WC raw material to obtain a first mixed material;

[0071] Adding a preset proportion of deoxidizer to the first mixed material to obtain a second mixed material;

[0072] Pressing the second mixed material into a mold to obtain a test block;

[0073] The test block is debonded and sintered to detect whether the sintered test block is carburized or decarburized; if it is not decarburized or carburized, it can directly enter mass production.

[0074] In some specific embodiments, the total C content in the WC raw material is in the range of 6.13%±0.02 by weight.

[0075] In some specific embodiments, the amount of the decarbonizer added is 0.26-0.47% of the WC raw material in terms of weight percentage; and the amount of the deoxidizer added is 4-8 g per 20 g of the first mixed material.

[0076] In some specific embodiments, the relative magnetic saturation value is calculated for the test block that is not decarburized or carburized, and the amount of the selected decarburizer and deoxidizer is determined by comparing the brand and other performance test values; then the carbon-oxygen balance of the cemented carbide is batch-controlled according to the amount of the decarburizer and deoxidizer obtained. For the test block that is decarburized or carburized, the preset ratio value is adjusted and the method steps are repeated until the test block that is not decarburized or carburized is obtained.

[0077] In some specific embodiments, a method for controlling the carbon-oxygen balance of cemented carbide comprises the following steps:

[0078] 1. Purchase WC saturated with C, with total C in the range of 6.13% ± 0.02.

[0079] 2. Add 0.47-0.26% TiO2 to the mixture, and divide 100g of the mixture mixed with TiO2 into five portions.

[0080] 3. Add 4, 5, 6, 7, and 8 g of rubber forming agent to five portions of the above mixture respectively.

[0081] 4. Press the material with molding agent added into test blocks.

[0082] 5. Debonding ~ sintering 4 test pieces.

[0083] 6. Check the fired test blocks: decarburization; calculate the relative magnetic saturation value of the non-decarburized and carburized test blocks, and determine the amount of forming agent and gold oxide to be selected by comparing the brand and other test values ​​(hardness, strength, fracture...).

[0084] 7. Infiltrate the molding agent and metal oxide in batches according to the amounts determined in 6, press the product → sinter.

[0085] In a fourth aspect, based on the same inventive concept, the present invention provides a method for recovering cemented carbide, the method comprising using the carbon-oxygen balance regulating composition for cemented carbide according to any one of the first aspects to recover the cemented carbide, the method comprising the following steps:

[0086] Determining the C content in WC in the scrap alloy material, and judging whether the scrap alloy material is saturated with C, lacking in C, or oversaturated with C;

[0087] Adding a decarburizing agent in a preset proportion to the waste alloy material lacking in carbon or being oversaturated in carbon to obtain a third mixed material;

[0088] Adding a preset proportion of a deoxidizer to the third mixed material to obtain a fourth mixed material;

[0089] Pressing and molding the fourth mixed material to obtain a test block;

[0090] The test block is debonded and sintered to detect whether the sintered test block is carburized or decarburized; if it is not decarburized or carburized, it can directly enter mass production.

[0091] In some specific embodiments, the objects of recycling cemented carbide do not include raw materials (WC), but are limited to recycled materials, including electrolytic recycling of WC; zinc dissolution method recycling of cemented carbide powder, crushed materials and other recycled materials.

[0092] In some specific embodiments, a method for recycling cemented carbide comprises the following steps:

[0093] 1. Determine the C content in WC in the scrap alloy. Determine whether it is saturated with C, lacking in C, or oversaturated with C.

[0094] 2. Collect representative samples for oxygen and C balance test:

[0095] ① Add 0.47-0.26% TiO2 to the mixture, and take five portions of the mixture mixed with TiO2, 100g each.

[0096] ②, add 4, 5, 6, 7, 8g of rubber forming agent to five parts of the mixture in ① respectively.

[0097] ③. Press the material with molding agent added into test blocks.

[0098] ④, debond and sinter the above ③ test blocks.

[0099] ⑤, Check the fired test blocks: decarburization; calculate the relative magnetic saturation value of the non-decarburized and carburized test blocks, and determine the amount of forming agent and gold oxide to be selected by comparing the brand and other test values ​​(hardness, strength, fracture...).

[0100] ⑥, batch infiltrate the molding agent and metal oxide according to the amount determined in step 6, press the product → sinter.

[0101] It should be noted that the operating steps involved in the carbon-oxygen balance regulating composition for cemented carbide provided in the embodiments of the present invention and its application, unless otherwise specified or explained, can be carried out in a conventional manner in the art or using existing equipment in the art, and will not be described one by one here.

[0102] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0103] Example 1

[0104] This example provides a carbon-oxygen balance regulating composition for cemented carbide, wherein the carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizing agent and a deoxidizing agent;

[0105] The decarburizing agent is a metal oxide; the metal oxide is tungsten trioxide;

[0106] The deoxidizer is a molding agent, the molding agent is a compression-molded rubber molding agent, and the compression-molded rubber molding agent is nitrile rubber.

[0107] Example 2

[0108] This example provides a carbon-oxygen balance regulating composition for cemented carbide, wherein the carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizing agent and a deoxidizing agent;

[0109] The decarburizing agent is a metal oxide; the metal oxide is titanium dioxide;

[0110] The deoxidizer is a molding agent, the molding agent is a compression-molded rubber molding agent, and the compression-molded rubber molding agent is butadiene rubber.

[0111] Example 3

[0112] This example provides a carbon-oxygen balance regulating composition for cemented carbide, wherein the carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizing agent and a deoxidizing agent;

[0113] The decarburizing agent is a metal oxide; the metal oxide is tungsten trioxide;

[0114] The deoxidizer is a molding agent, the molding agent is a mixed molding agent of injection molding and extrusion molding, and the mixed molding agent of injection molding and extrusion molding is paraffin.

[0115] Example 4

[0116] This example provides a carbon-oxygen balance regulating composition for cemented carbide, wherein the carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizing agent and a deoxidizing agent;

[0117] The decarburizing agent is a metal oxide; the metal oxide is titanium dioxide;

[0118] The deoxidizer is a molding agent, the molding agent is a mixed molding agent of injection molding and extrusion molding, and the mixed molding agent of injection molding and extrusion molding is paraffin.

[0119] Example 5

[0120] This example provides a method for recycling cemented carbide, taking ZT10 cemented carbide as an example, wherein ZT10 is a recycled material of zinc melting waste alloy; the method comprises the following steps:

[0121] 1. Determine the C content in WC in the scrap alloy. Determine whether it is saturated with C, lacking in C, or oversaturated with C.

[0122] 2. Collect representative samples for oxygen and C balance test:

[0123] ① Add 0.47-0.26% TiO2 to the mixture, and take five portions of the mixture mixed with TiO2, 100g each.

[0124] ②, add 4, 5, 6, 7, 8g of rubber forming agent to five parts of the mixture in ① respectively.

[0125] ③. Press the material with molding agent added into test blocks.

[0126] ④, debond and sinter the above ③ test blocks.

[0127] ⑤, Check the fired test blocks: decarburization; calculate the relative magnetic saturation value of the non-decarburized and carburized test blocks, and determine the amount of forming agent and gold oxide to be selected by comparing the brand and other test values ​​(hardness, strength, fracture...).

[0128] ⑥, batch infiltrate the molding agent and metal oxide according to the amount determined in step 6, press the product → sinter.

[0129] The specific dosages of the deoxidizer (i.e., molding agent, specifically paraffin wax) and the decarburizer (i.e., titanium dioxide, titanium dioxide) and the experimental results are shown in Table 1.

[0130] Table 1

[0131] Forming agent g Titanium dioxide g density hardness Decarbonization carburization Metallography 6.5 0.26 14.26 90.6~90.9 none none A02B02C00 7.5 0.26 14.21 90.6~91.1 none none A02B02C00 8.5 0.26 14.21 90.8~91 none none A02B02C00 9.5 0.26 14.21 90.5~91.1 none Slight carburization A02B02C00

[0132] Example 6

[0133] This example provides a method for recycling cemented carbide, taking BT15N22-93 cemented carbide as an example, wherein BT15N22-93 is an electrolytically recycled waste alloy material; the method comprises the following steps:

[0134] 1. Determine the C content in WC in the scrap alloy. Determine whether it is saturated with C, lacking in C, or oversaturated with C.

[0135] 2. Collect representative samples for oxygen and C balance test:

[0136] ① Add 0.47-0.26% TiO2 to the mixture, and take five portions of the mixture mixed with TiO2, 100g each.

[0137] ②, add 4, 5, 6, 7, 8g of rubber forming agent to five parts of the mixture in ① respectively.

[0138] ③. Press the material with molding agent added into test blocks.

[0139] ④, debond and sinter the above ③ test blocks.

[0140] ⑤, Check the fired test blocks: decarburization; calculate the relative magnetic saturation value of the non-decarburized and carburized test blocks, and determine the amount of forming agent and gold oxide to be selected by comparing the brand and other test values ​​(hardness, strength, fracture...).

[0141] ⑥, batch infiltrate the molding agent and metal oxide according to the amount determined in step 6, press the product → sinter.

[0142] The specific dosages of the deoxidizer (i.e., molding agent, specifically paraffin wax) and the decarburizer (i.e., titanium dioxide, titanium dioxide) and the experimental results are shown in Tables 2 and 3.

[0143] Table 2

[0144]

[0145] Table 3

[0146]

[0147]

[0148] Example 7

[0149] This example provides a method for recycling cemented carbide, taking BT15N22-113 cemented carbide as an example. The method includes the following steps which are the same as those in Example 6.

[0150] The specific dosage and experimental results of the deoxidizer (i.e., molding agent, specifically paraffin) and the decarburizer (i.e., titanium dioxide; the amount of titanium dioxide added in all experimental numbers is: 8.8 grams of titanium dioxide added to 1000 grams of material) are shown in Table 4.

[0151] Table 4

[0152] Serial number Molding dosage g density hardness Decarbonization carburization Metallography Porosity 1 4 13.825 89.5-90.6 no no A02B02C00 25-75:25 2 5.8 13.7592 89.5-90.6 no no A02B02C00 25-75:6 3 7 13.767 89.5-90.6 no no A02B02C00 25-125:1 4 8.5 13.7466 - no carburization - - 5 9.5 13.6913 - no carburization - - 6 10.5 13.6897 - no carburization - - 7 11.5 13.5711 - no carburization - - 8 12.5 13.5756 - no carburization - -

[0153] In summary, the embodiments of the present invention provide a carbon-oxygen balance regulating composition for cemented carbide. On the one hand, the present invention uses metal oxide as a decarburizing agent, which can more effectively solve the C problem in the carburizing and decarburizing molding agent, and the dosage is small, the cost is low, and the time is saved. On the other hand, the present invention uses a molding agent as a deoxidizing agent, which not only achieves deoxidation, but also the residual carbon in the molding agent can solve the problem of C deficiency in the alloy. The present invention achieves carbon-oxygen balance by adjusting the reasonable matching amount of metal oxide and molding agent. It can solve both carburizing and decarburization problems, and has a universal effect. Magnetic saturation measurement can also be used to solve the problem of precise carbon control. Obviously, the quality of the alloy has a higher control accuracy, which makes up for the shortcomings of the prior art.

[0154] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0155] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A carbon-oxygen balance regulating composition for cemented carbide, characterized in that: The carbon-oxygen balance regulating composition for cemented carbide comprises a decarburizer and a deoxidizer; The decarburizing agent is a metal oxide; The deoxidizer is a molding agent.

2. The carbon-oxygen balance regulating composition for cemented carbide according to claim 1, characterized in that: The metal oxide includes at least one of tungsten trioxide and titanium dioxide.

3. The carbon-oxygen balance adjusting composition for cemented carbide according to claim 1, characterized in that: The molding agent includes a compression-molded rubber molding agent and a mixed molding agent for injection molding and extrusion molding; the compression-molded rubber molding agent includes at least one of organic rubber and polymer resin rubber, and the mixed molding agent for injection molding and extrusion molding includes at least one of paraffin, polyethylene, and a dispersant.

4. Use of the carbon-oxygen balance regulating composition for cemented carbide according to any one of claims 1 to 3 in controlling the carbon-oxygen balance of cemented carbide and recovering cemented carbide.

5. A method for controlling the carbon-oxygen balance of cemented carbide, characterized in that: The method comprises using the carbon-oxygen balance regulating composition for cemented carbide according to any one of claims 1 to 3 to regulate the carbon-oxygen balance of cemented carbide, and the method comprises the following steps: Purchase saturated carbon tungsten carbide, including raw materials and recycled materials; perform carbon content analysis and calculation for WC with unknown carbon content, determine the carbon content in WC, and use it as a data reference for adding carbon-oxygen balance adjustment composition for cemented carbide; Adding a preset proportion of decarburizing agent to the WC raw material to obtain a first mixed material; Adding a preset proportion of deoxidizer to the first mixed material to obtain a second mixed material; Pressing the second mixed material into a mold to obtain a test block; The test block is debonded and sintered to detect whether the sintered test block is carburized or decarburized; if not, the test block is directly put into mass production.

6. The method for controlling carbon-oxygen balance of cemented carbide according to claim 5, characterized in that: Calculated in weight percentage, the total C content in the WC raw material is within the range of 6.13%±0.

02.

7. The method for controlling the carbon-oxygen balance of cemented carbide according to claim 5, characterized in that Saturated WC: 1) the amount of the decarburizer added is 0.2-1.0wt% of the total amount of the mixture; 2) the amount of the binder added in the molding agent is 0.9-1.3wt% of the mixture; For unsaturated C WC: 1) the amount of oxidant added is determined according to the C saturation degree of WC; 2) the amount of binder added in the molding agent is 0.9-1.3wt% of the mixture.

8. The method for controlling carbon-oxygen balance of cemented carbide according to claim 5, characterized in that: The relative magnetic saturation value of the non-decarburized and carburized test blocks is calculated, and the amount of the selected decarburizer and deoxidizer is determined by comparing the brand and other performance test values; then the carbon-oxygen balance of the cemented carbide is batch-controlled based on the obtained amount of decarburizer and deoxidizer, and then mass production is started after the control.

9. A method for recovering cemented carbide, characterized in that: The method comprises using the carbon-oxygen balance regulating composition for cemented carbide according to any one of claims 1 to 3 to recover cemented carbide, and the method comprises the following steps: Determining the C content in WC in the scrap alloy material, and judging whether the scrap alloy material is saturated with C, lacking in C, or oversaturated with C; Adding a decarburizing agent in a preset proportion to the waste alloy material lacking in carbon or being oversaturated in carbon to obtain a third mixed material; Adding a preset proportion of a deoxidizer to the third mixed material to obtain a fourth mixed material; Pressing and molding the fourth mixed material to obtain a test block; The test block is debonded and sintered to detect whether the sintered test block is carburized or decarburized; if not, the test block is directly put into mass production.