Anodic oxidation 5-series aluminum alloy material as well as preparation method and application thereof
By adjusting the composition and hot rolling process of aluminum alloy, the problems of poor surface morphology and low yield of anodized 5-Series aluminum alloy materials are solved, and the effects of no different color stripes on the surface, high white brightness and uniform grains are achieved, satisfying the High-end usage requirements for 3C products.
Patent Information
- Application Number
- CN202411148204.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The anodized 5-type aluminum alloy material in the prior art is poor in surface morphology after chemical casting and anodizing treatment, low yield, coarse grains and uneven distribution, which cannot meet the surface decoration and structural parts of 3C products. High-end usage requirements.
By adjusting the composition and hot rolling process of aluminum alloy, including multiple hot rolling and cold rolling, and performing intermediate annealing and heat treatment during the process, we ensure that the impurity content of the aluminum alloy material is low and the grain size is small and uniform, and avoiding impurity phases with deterioration in performance Precipitation, a hot rolling process with a large pressure amount is used to increase the grain boundary to form more nucleated particles, so as to achieve no different color stripes on the surface and high white brightness.
The surface of the anodized 5-Series aluminum alloy material has no different color stripes defects, high white brightness and uniform grain size, which meets the usage requirements of high-end 3C products, and improves yield and production efficiency.
Smart Images

Figure CN119040702A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an anodized 5-series aluminum alloy material, a preparation method thereof and applications thereof. Background Art
[0002] Aluminum alloy has many advantages such as high strength, good plasticity and toughness, and can be anodized. In recent years, the application market in the 3C field has continued to expand, making it the best choice for structural materials and surface materials for 3C (computers, communications and consumer electronics products). 3C aluminum materials are usually made of aluminum alloy ingots, which are rolled into plates and strips of a certain thickness, and then stamped and CNC (computer numerical control) processed into the required products. Since 3C surface materials not only require rolled aluminum alloy materials to have good strength and forming properties, but also have higher requirements for surface properties, the materials used are not allowed to have different color material lines on the surface after chemical polishing and anodizing, and the white brightness is high.
[0003] However, the 3C aluminum materials in the prior art not only have different-color stripe defects on the surface after chemical polishing and anodizing, but also have a large number of rolling passes, which greatly reduces the yield and production efficiency, thus seriously restricting its application development in this field.
[0004] Based on this, how to provide an anodized 5 series aluminum alloy material and design its component ratio and corresponding preparation process conditions so that it can have excellent surface properties and a finer and more uniform internal grain structure to better meet the use requirements of 3C aluminum alloys is one of the important technical problems that need to be solved in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide an anodized 5 series aluminum alloy material, a preparation method and application thereof, so as to solve the problems of poor surface morphology and low yield of the anodized 5 series aluminum alloy material in the prior art after chemical polishing and anodizing treatment.
[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing an anodized 5-series aluminum alloy material, comprising: step S1, preparing raw materials: in terms of weight percentage, the composition of the anodized 5-series aluminum alloy material includes 0-0.04% Si, 0-0.06% Fe, 1.8%-3.5% Mn, 0.01%-0.04% Ti, and does not contain Cu, and the balance is Al and unavoidable impurity elements, and the raw materials are prepared according to the composition of the anodized 5-series aluminum alloy material; step S2, melting and casting: the raw materials are sequentially melted and cast to obtain an ingot; step S 3. Hot rolling: the ingot is hot rolled at least 5 times, and the reduction amount of each hot rolling is independently 40mm to 70mm to obtain a hot rolled material; step S4, cold rolling: the hot rolled material is cold rolled for multiple times, and the multiple cold rolling processes include at least one intermediate annealing, and each intermediate annealing is arranged between two adjacent cold rollings to obtain a cold rolled material; step S5, finished product heat treatment: the cold rolled material is heat treated to obtain a heat treated material; step S6, surface treatment: the heat treated material includes surface treatment, and the surface treatment includes anodizing treatment to obtain anodized 5 series aluminum alloy material.
[0007] Furthermore, the number of hot rolling in step S3 does not exceed 12 times, and the reduction amount of each hot rolling is independently 60 mm to 70 mm.
[0008] Furthermore, in step S3, the final rolling thickness of the hot rolling is 6 mm to 9 mm; preferably, the initial rolling thickness of the hot rolling is 500 mm to 600 mm, and the final rolling thickness is 8 mm to 9 mm.
[0009] Furthermore, in step S3, the starting temperature of hot rolling is 475°C to 485°C, and the finishing temperature is 270°C to 285°C.
[0010] Furthermore, before hot rolling in step S3, the ingot obtained in step S2 is kept warm at a temperature of 500°C to 510°C.
[0011] Furthermore, the total cold rolling rate of the multiple cold rolling processes is 80% to 90%; preferably, when the total cold rolling rate of the multiple cold rolling processes reaches 55% to 80%, intermediate annealing is performed.
[0012] Furthermore, the multiple cold rolling process includes two intermediate annealings, and when the total cold rolling rate of the multiple cold rolling reaches 55-65%, the first intermediate annealing is performed, and when the total cold rolling rate of the multiple cold rolling reaches 75-80%, the second intermediate annealing is performed.
[0013] Furthermore, the temperature of each intermediate annealing is independently 300° C. to 360° C., and the holding time is independently 1 h to 3 h.
[0014] Furthermore, the heat treatment temperature in step S5 is 160° C. to 220° C., and the heat preservation time is 1 h to 3 h.
[0015] The second aspect of the present invention provides an anodized 5-series aluminum alloy material, which is prepared by the above-mentioned preparation method of the anodized 5-series aluminum alloy material, and the surface of the obtained anodized 5-series aluminum alloy material has no heterochromatic stripe defects, and the white brightness L value is ≥90.
[0016] Furthermore, the surface grain size of the anodized 5-series aluminum alloy material is 20 to 40 μm, and the grain size of the cross section of the material is 15 to 30 μm.
[0017] A third aspect of the present invention provides an application of the above-mentioned anodized 5-series aluminum alloy material as a structural material and / or surface material in the fields of computers, communications and consumer electronic products.
[0018] By applying the technical solution of the present invention, the problem of low white brightness and coarse and unevenly distributed grains of 5xxx aluminum alloy materials after anodization is solved. By focusing on regulating the aluminum alloy composition and hot rolling process, the finished aluminum alloy material has low impurity content and small and uniform grain size. The anodized 5 series aluminum alloy material obtained after chemical polishing and anodizing has no heterochromatic stripe defects on the surface and high white brightness, meeting the technical requirements for the use of surface decorative materials and internal structural materials of high-end 3C products. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0020] Figure 1 This is a metallographic coating photograph of the cross section of the hot-rolled plate in Example 1;
[0021] Figure 2 This is a metallographic coating photograph of the cross section of the hot-rolled plate in Comparative Example 4;
[0022] Figure 3 This is the grain distribution diagram of the anodized 5-series aluminum alloy material finally obtained in Example 1;
[0023] Figure 4 This is the grain distribution diagram of the anodized 5-series aluminum alloy material finally obtained in Comparative Example 4. DETAILED DESCRIPTION
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0025] As described in the background technology, the anodized 5 series aluminum alloy materials in the prior art have the problems of poor surface morphology and low yield after chemical polishing and anodizing. In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing an anodized 5 series aluminum alloy material, comprising: step S1, preparing raw materials: in terms of weight percentage, the composition of the anodized 5 series aluminum alloy material includes 0-0.04% Si, 0-0.06% Fe, 1.8%-3.5% Mn, 0.01%-0.04% Ti, and does not contain Cu, and the balance is Al and unavoidable impurity elements, and the raw materials are prepared according to the composition of the anodized 5 series aluminum alloy material; step S2, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S3, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S4, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S5, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S6, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S7, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S8, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S9, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S10, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S11, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S12, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S13, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; step S14, melting and casting: the raw materials are melted and cast in sequence to obtain an ingot; S3, hot rolling: the ingot is hot rolled at least 5 times, and the reduction amount of each hot rolling is independently 40mm to 70mm, so as to obtain a hot rolled material; step S4, cold rolling: the hot rolled material is cold rolled for multiple times, and the multiple cold rolling processes include at least one intermediate annealing, and each intermediate annealing is arranged between two adjacent cold rollings, so as to obtain a cold rolled material; step S5, finished product heat treatment: the cold rolled material is heat treated to obtain a heat treated material; step S6, surface treatment: the heat treated material is subjected to surface treatment, and the surface treatment includes anodizing treatment to obtain anodized 5 series aluminum alloy material.
[0026] The preparation method of the above-mentioned anodized 5 series aluminum alloy material provided by the present invention aims at the problem that the white brightness of the 5 series aluminum alloy material is low after anodization, and the grains are coarse and unevenly distributed. By focusing on regulating the aluminum alloy composition and hot rolling process, the finished aluminum alloy material has low impurity content and small and uniform grain size. Its main steps include smelting, casting, heating, multiple hot rolling, multiple cold rolling, finished product annealing heat treatment and final surface treatment. In the design process of the above-mentioned alloy composition, the inventor has coordinated and comprehensively controlled the content of each element therein through a large number of experiments, so that in the subsequent multiple hot rolling and multiple cold rolling processes, each strengthening element is dissolved in the matrix to the maximum extent to achieve the purpose of strengthening. At the same time, the precipitation of impurity phases that deteriorate the performance is well avoided, ensuring the various performances of the obtained aluminum alloy material, especially the 5 series (same as 5xxx) aluminum alloy.
[0027] Also, the anodized 5 series aluminum alloy material provided by the present invention does not include the Cu metal element, because the inventors have found through a large number of experiments and comparisons that for the alloy composition formula and the corresponding preparation process provided by the present invention, if the Cu element is added alone or in combination on the basis of it, it will no longer be perfectly compatible with the above-mentioned preparation method, thereby bringing certain negative effects. Although in the field of aluminum alloys, the Cu element can improve the strength and thermal stability of the alloy, but for the above-mentioned formula provided by the present invention. Cu will make the oxide film reddish, increase the defects of the oxide film, and thus affect the surface properties. The preparation method provided by the present invention, for the above-mentioned alloy formula, strictly maintains multiple passes and large reduction (40mm~70mm) rolling during multiple hot rolling processes, and performs one or more intermediate annealing during multiple cold rolling processes, so as to better adapt to the above-mentioned alloy formula, and comprehensively improve the surface quality and internal grain morphology of the obtained material, specifically:
[0028] Conventional industrial pure aluminum (Fe about 0.14-0.18%, Si about 0.06%) is generally used in the prior art to prepare 5 series aluminum materials. However, due to the high content of Fe and Si in the raw material, a large number of micron-level iron-rich and silicon-rich Al-Fe-Si second phase compounds are generally present in the resulting alloy structure. Therefore, the prior art often uses a particle stimulated nucleation mechanism (Particle Stimulated Nucleation-PSN mechanism) to promote recrystallization during alloy annealing, increase the nucleation rate, and play a role in grain refinement. However, in order to optimize the surface morphology, that is, to further improve the surface quality and anodizing performance of 3C aluminum materials, it is necessary to prepare 5-series aluminum materials with higher purity (Fe≤0.07%, Si≤0.04%). Therefore, the trace amount of Fe and Si is not enough to form enough Al-Fe-Si second phase compounds to start the PSN mechanism. Therefore, the recrystallization mechanism of high-purity 5-series aluminum materials is mainly based on the grain boundary nucleation mechanism, that is, a small section of the grain boundary will suddenly bow to the side with high dislocation density to form a recrystallization core. This process is also called strain-induced grain boundary migration.
[0029] In view of the above situation, the present invention adopts a process of multiple and large reductions during hot rolling to produce more grain boundaries, so that the material after hot rolling has higher deformation energy storage, and under the leading role of the grain boundary nucleation mechanism, more grain boundaries form more nucleation particles. At this time, since there is not enough space for the grains to grow unevenly, more uniform and fine grains are eventually generated, so that the plate has high white brightness and no heterochromatic stripes after anodization. However, conventional, especially smaller pass reductions cannot achieve a good grain refinement effect, and the grain distribution is uneven, and heterochromatic stripes appear on the surface after anodization, affecting the surface properties of the plate.
[0030] Of course, it needs to be additionally explained that the above steps provided by the present invention, in addition to the advantages of improving the alloy performance themselves, are more importantly designed based on the above-mentioned specific metal element formula, and the steps can cooperate with each other, that is, as an overall solution, to achieve the improvement of the comprehensive performance of the aluminum alloy material, especially the surface morphology.
[0031] On the basis of the above contents, for the alloy formula provided by the present invention, taking into account the surface performance of the obtained aluminum alloy material, the inventors further preferred the reduction amount for each hot rolling to be 60mm to 70mm after a large number of experiments, and simultaneously coordinated the preferred number of hot rolling to be no more than 10 times, so as to maximize the surface brightness of the obtained aluminum alloy material and optimize its surface morphology.
[0032] Furthermore, in order to better match the prepared aluminum alloy material with its preparation method, the final rolling thickness of the hot rolling in step S3 is preferably 6mm to 9mm. At the same time, the inventor further preferred the final rolling thickness of the hot rolling to be 8mm to 9mm after a large number of experiments, so that more grain boundaries can be generated inside the structure of the obtained hot-rolled material through the above-mentioned multiple and large-reduction hot rolling, thereby obtaining more nucleation points and finally forming more uniform and fine grains, further improving the various properties of the material, especially the surface properties. Specifically, the initial rolling thickness is 400mm to 800mm.
[0033] In order to optimize the plastic deformation ability and dimensional accuracy of the aluminum alloy material, and to suppress the occurrence of defects such as different color stripes and even potholes and wrinkles on its surface, in several typical implementations, the starting temperature of the hot rolling in step S3 is preferably 475°C to 485°C, and the final rolling temperature is 270°C to 285°C.
[0034] Since the temperature of the material will inevitably drop during the actual hot rolling process, in order to minimize the stress increase caused by its rapid cooling while reducing mass loss and surface defects, the preparation method provided by the present invention further includes keeping the ingot obtained in step S2 warm before hot rolling in step S3, and the preferred keeping temperature is 500°C to 510°C after a large number of experiments.
[0035] In several typical embodiments, the inventors rely on the aluminum alloy composition formula adopted and the previous hot rolling conditions, and after a large number of experiments, the inventors optimize step S4. When the total cold rolling rate of multiple cold rolling reaches 55% to 80%, intermediate annealing is performed to obtain intermediate annealed materials, and the intermediate annealed materials are subjected to the next cold rolling; at the same time, the temperature of each intermediate annealing is preferably independently 300°C to 360°C, and the holding time is independently 1h to 3h. The intermediate annealing is preferably performed when the total cold rolling rate reaches 55% to 80%, and the condition parameters are coordinated as above, which can more effectively improve the plasticity of the aluminum alloy material during cold working, especially for the hot-rolled material obtained by multiple high-pressure hot rolling provided by the present invention, which can more significantly improve the internal grain structure of the material and weaken its internal stress, thereby obtaining a cold-rolled sheet with fewer surface defects, higher appearance quality, and more suitable for subsequent surface treatment. On this basis, the inventors further optimize the total cold rolling rate of multiple cold rolling to be 80% to 90%, so as to better balance the thickness uniformity and surface quality of the obtained aluminum alloy material.
[0036] In several typical implementations, the multiple cold rolling process includes two intermediate annealings, and when the total cold rolling rate of the multiple cold rolling reaches 55-65%, the first intermediate annealing is performed, and when the total cold rolling rate of the multiple cold rolling reaches 75-80%, the second intermediate annealing is performed. After a large number of experiments, the inventors have optimized the above-mentioned cold rolling and intermediate annealing matching scheme to better match the aluminum alloy material formula provided, thereby obtaining a 5 series aluminum alloy material with better comprehensive performance, especially more uniform and fine grains, and better surface performance after subsequent chemical polishing and anodizing treatment.
[0037] Furthermore, in order to adapt to the aluminum alloy material obtained by the above-mentioned hot rolling and cold rolling treatment, the heat treatment temperature in step S5 is preferably 160°C to 220°C, and the holding time is 1h to 3h, so as to better eliminate residual stress, homogenize its internal structure, optimize grain size, and improve surface morphology.
[0038] The second aspect of the present invention provides an anodized 5-series aluminum alloy material, which is prepared by the above-mentioned method for preparing anodized 5-series aluminum alloy material, and the surface of the obtained anodized 5-series aluminum alloy material has no heterochromatic stripe defects, and the white brightness L value is ≥ 90. The obtained anodized 5-series aluminum alloy material exhibits extremely high surface quality, and also has good purity and internal grain structure.
[0039] In several preferred embodiments, the surface grain size of the anodized 5-series aluminum alloy material is 20-40 μm, and the grain size of the cross-section of the material is 15-30 μm. The obtained anodized 5-series aluminum alloy material has fine surface grains and uniform internal grain size distribution, so it can not only meet the requirements of surface quality rate well, but also has good mechanical properties, especially plasticity.
[0040] The anodized 5-series aluminum alloy material provided by the present invention can be a strip or a plate so as to better meet the use requirements in various fields.
[0041] The third aspect of the present invention provides an application of the above-mentioned anodized 5-series aluminum alloy material as a structural material and / or surface material in the fields of computers, communications and consumer electronic products. The above-mentioned anodized 5-series aluminum alloy material provided by the present invention has fine internal grain structure and high uniformity. After chemical polishing and anodizing treatment, the surface is smooth and defect-free, and has high brightness and whiteness, which can well adapt to various fields, especially the high standards and high requirements of related products in the 3C field. At the same time, the anodized 5-series aluminum alloy material has high production efficiency, high yield rate, and low production cost, so it has high application value.
[0042] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0043] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0044] Example 1
[0045] A method for preparing anodized 5 series aluminum alloy material:
[0046] Step S1, preparing raw materials: preparing alloy composition as follows: Si=0.03%, Fe=0.04%, Mg=2.46%, Ti=0.012%, and the balance of Al and unavoidable impurities (the composition is the same as that in Table 1);
[0047] Step S2, melting and casting: according to the above-mentioned component ratio, pure aluminum ingots and pure magnesium ingots are added in proportion to melt into aluminum liquid, Ti is added online in the form of Al-Ti-B wire, and finally an aluminum alloy flat ingot, i.e., an ingot, is prepared; the ingot is heated to 505°C in a furnace for insulation.
[0048] Step S3, hot rolling: start rolling temperature 475℃, keep 6 passes with a reduction of 40-70mm per pass, final rolling temperature 275℃, finally obtain hot rolled material with a final thickness of 8.5mm; wherein the reduction of the 6 passes is 50mm, 60mm, 70mm, 70mm, 70mm and 60mm respectively. The metallographic coating photo of the cross section of the hot rolled plate obtained at this time is shown in Figure 1 , Figure 1 a, b, c and d are grain distribution diagrams at different positions from one surface to another of the obtained hot-rolled plate.
[0049] Step S4, cold rolling: perform twelve cold rollings with a total cold rolling rate of 85%, and perform intermediate annealing once when the total cold rolling rate reaches 58% and when the total cold rolling rate reaches 79%, respectively. The intermediate annealing conditions are 320°C and 2h to obtain a cold-rolled material.
[0050] Step S5, heat treatment of finished product: heat treatment of the cold-rolled material at an annealing temperature of 180° C. and a holding time of 2 h to obtain a heat-treated material.
[0051] Step S6, surface treatment: chemical polishing and anodizing treatment are performed on the heat-treated material to obtain an anodized 5 series aluminum alloy material, the grain distribution diagram of which is shown in FIG. Figure 3 Among them, the chemical polishing uses a mixed solution of phosphoric acid and sulfuric acid at 80°C for 60s, and the anodizing treatment uses a sulfuric acid solution at 30°C for 20min.
[0052] Example 2
[0053] A preparation method of anodized 5 series aluminum alloy material:
[0054] Step S1, preparing raw materials: preparing alloy composition as follows: Si=0.03%, Fe=0.05%, Mg=3.31%, Ti=0.032%, and the balance of Al and unavoidable impurities (the composition is the same as that in Table 1);
[0055] Step S2, melting and casting: melting and casting according to the method in Example 1 to obtain an ingot; heating the ingot in a furnace to 508° C. and keeping it warm.
[0056] Step S3, hot rolling: the starting rolling temperature is 480°C, and the reduction in each pass is maintained at 7 passes with a reduction of 40 to 70 mm. The final rolling temperature is 285°C, and finally a hot-rolled material with a final rolling thickness of 8 mm is obtained; the reductions in the 7 passes are 45 mm, 50 mm, 60 mm, 60 mm, 65 mm, 65 mm and 55 mm respectively.
[0057] Step S4, cold rolling: perform cold rolling twelve times with a total cold rolling rate of 88%, and perform an intermediate annealing when the total cold rolling rate reaches 61%, the intermediate annealing conditions are 345°C, 1h, to obtain a cold rolled material.
[0058] Step S5, heat treatment of finished product: heat treatment of the cold-rolled material at an annealing temperature of 200° C. and a holding time of 2 h to obtain a heat-treated material.
[0059] Step S6, surface treatment: chemically polishing and anodizing the heat-treated material according to the method in Example 1 to obtain an anodized 5 series aluminum alloy material.
[0060] Example 3
[0061] A preparation method of anodized 5 series aluminum alloy material:
[0062] Step S1, preparing raw materials: the same as in Example 1;
[0063] Step S2, melting and casting: melting and casting according to the method in Example 1 to obtain an ingot; heating the ingot in a furnace to 500° C. and keeping it warm.
[0064] Step S3, hot rolling: the starting rolling temperature is 460°C, and the rolling reduction is maintained at 40-70 mm for 5 passes, and the final rolling temperature is 268°C, and finally a hot-rolled material with a final rolling thickness of 8.5 mm is obtained; wherein the rolling reductions for the 5 passes are 50 mm, 65 mm, 70 mm, 70 mm and 65 mm respectively.
[0065] Step S4, cold rolling: cold rolling is performed ten times with a total cold rolling rate of 83%, and an intermediate annealing is performed when the total cold rolling rate reaches 57%, and the intermediate annealing conditions are 305° C. and 2.5 h to obtain a cold rolled material.
[0066] Step S5, heat treatment of finished product: heat treatment of the cold-rolled material at an annealing temperature of 250° C. and a holding time of 1 h to obtain a heat-treated material.
[0067] Step S6, surface treatment: chemically polishing and anodizing the heat-treated material according to the method in Example 1 to obtain an anodized 5 series aluminum alloy material.
[0068] Example 4
[0069] A preparation method of anodized 5 series aluminum alloy material:
[0070] The difference between this embodiment and embodiment 1 is only the starting rolling temperature and the final rolling temperature in step S3, specifically: the starting rolling temperature is 490° C., the final rolling temperature is 290° C., and the other conditions are the same.
[0071] Example 5
[0072] A method for preparing anodized 5 series aluminum alloy material:
[0073] The difference between this embodiment and embodiment 1 is only in step S3, specifically: maintaining 6 passes with a reduction of 70 mm in each pass, and finally obtaining a hot-rolled material with a final rolling thickness of 7 mm; the starting rolling temperature and the final rolling temperature conditions are the same as those in embodiment 1.
[0074] Example 6
[0075] A method for preparing anodized 5 series aluminum alloy material:
[0076] The difference between this embodiment and embodiment 1 is only in step S3, specifically: maintaining 6 passes with a reduction of 55 mm in each pass, and finally obtaining a hot-rolled material with a final rolling thickness of 5 mm; the starting rolling temperature and the final rolling temperature conditions are the same as those in embodiment 1.
[0077] Example 7
[0078] A method for preparing anodized 5 series aluminum alloy material:
[0079] The difference between this embodiment and embodiment 1 is only in step S3, specifically: maintaining 10 passes with a reduction of 66 mm in each pass, and finally obtaining a hot-rolled material with a final rolling thickness of 10 mm; the starting rolling temperature and the final rolling temperature conditions are the same as those in embodiment 1.
[0080] Example 8
[0081] A method for preparing anodized 5 series aluminum alloy material:
[0082] The difference between this embodiment and embodiment 1 is only in step S2, specifically: after the ingot is obtained, no heat preservation treatment is performed, but it is allowed to cool naturally, and then the subsequent steps are performed.
[0083] Example 9
[0084] A method for preparing anodized 5 series aluminum alloy material:
[0085] The difference between this embodiment and embodiment 2 is only in step S4, specifically: twelve cold rollings are performed with a total cold rolling rate of 88%, and an intermediate annealing is performed when the total cold rolling rate reaches 82%, and the conditions of the intermediate annealing are 345°C and 1h.
[0086] Example 10
[0087] A method for preparing anodized 5 series aluminum alloy material:
[0088] The difference between this embodiment and embodiment 3 is only in step S4, specifically: performing ten cold rollings with a total cold rolling rate of 83%, and performing an intermediate annealing when the total cold rolling rate reaches 50%, and the conditions of the intermediate annealing are 305°C and 2.5h.
[0089] The difference between Comparative Examples 1 to 3 and Example 1 is that the composition ratios of the anodized 5-series aluminum alloy materials are different, see Table 1 for details.
[0090] Comparative Example 4
[0091] A method for preparing anodized 5 series aluminum alloy material:
[0092] The difference between this comparative example and Example 1 is only in step S3, specifically: the starting rolling temperature and the final rolling temperature are the same, but the reduction of each pass is maintained at 30 mm for 3 passes, and finally a hot-rolled material with a final rolling thickness of 8 mm is obtained. The grain distribution diagram of the hot-rolled material obtained at this time is shown in FIG. Figure 2 , Figure 2 a, b, c and d are the grain distribution diagrams of different positions from one surface to another of the hot rolled plate. The grain distribution diagram of the final material product is shown in Figure 4 .
[0093] Comparative Example 5
[0094] A method for preparing anodized 5 series aluminum alloy material:
[0095] The difference between this comparative example and Example 1 is only in step S3, specifically: the starting rolling temperature, the final rolling temperature and the starting rolling thickness are consistent, but the reduction amount of each pass is maintained at 30 mm for 15 passes, and finally a hot-rolled material with a final rolling thickness of 8.5 mm is obtained.
[0096] Comparative Example 6
[0097] A method for preparing anodized 5 series aluminum alloy material:
[0098] The difference between this comparative example and Example 1 is only in step S3, specifically: the starting rolling temperature, the final rolling temperature and the starting rolling thickness are consistent, but the reduction amount of each pass is maintained at 80 mm for 3 passes, and finally a hot-rolled material with a final rolling thickness of 8.5 mm is obtained.
[0099] Comparative Example 7
[0100] A method for preparing anodized 5 series aluminum alloy material:
[0101] The only difference between this comparative example and Example 1 is that no intermediate annealing is performed in the cold rolling process in step S4.
[0102] Test Method
[0103] Grain size: The surface average grain size and cross-sectional average grain size of the obtained anodized 5 series aluminum alloy material were tested according to GBT 3246.1-2012.
[0104] White brightness: According to GB / T 12967.6-2022, using integrating sphere spectrophotometer d / 8, light source D65, test aperture 25mm, observer angle 10°; test mode uses SCI: including specular reflection mode.
[0105] The above tests were performed on the aluminum alloy materials obtained in each embodiment and comparative example, and the obtained results are shown in Table 2.
[0106] Table 1
[0107]
[0108]
[0109] And, in Comparative Example 3, 1.5% of Cu was further added.
[0110] Table 2
[0111] Surface average grain size / μm Average grain size of cross section / μm Surface color stripe defect L value Example 1 25 17 none 95 Example 2 28 19 none 93 Example 3 32 23 none 90 Example 4 31 25 none 91 Example 5 29 21 none 92 Example 6 35 28 none 90 Example 7 37 29 none 92 Example 8 29 22 none 90 Example 9 29 23 none 91 Example 10 36 27 none 91 Comparative Example 1 48 41 Yes, a small amount 82 Comparative Example 2 51 45 Yes, a small amount 83 Comparative Example 3 49 40 Yes, a small amount 85 Comparative Example 4 57 42 Yes, a lot 73 Comparative Example 5 54 38 Yes, a lot 79 Comparative Example 6 48 37 Yes, a lot 72 Comparative Example 7 53 46 Yes, a lot 78
[0112] From the above description, it can be seen that the above-mentioned embodiment of the present invention realizes the preparation of anodized 5-series aluminum alloy materials with low impurity content, fine and uniform grain size, no heterochromatic stripe defects on the surface, and high white brightness.
[0113] Specifically, conventional industrial pure aluminum (Fe about 0.14 ~ 0.18%, Si about 0.06%) is used to prepare 5xxx aluminum. Due to the high content of Fe and Si, there are more micron-level iron-rich and silicon-rich Al-Fe-Si second phase compounds in the alloy structure, which can promote recrystallization during alloy annealing through the particle stimulated nucleation mechanism (Particle Stimulated Nucleation-PSN mechanism), increase the nucleation rate, and play a role in grain refinement. In order to further improve the surface quality and anodizing performance of 3C aluminum materials, it is necessary to prepare 5xxx aluminum materials with higher purity (Fe≤0.07%, Si≤0.04%), but trace amounts of Fe and Si are not enough to form enough Al-Fe-Si second phase compounds to start the PSN mechanism. Therefore, the recrystallization mechanism of high-purity 5xxx aluminum is mainly based on the grain boundary arch nucleation mechanism, that is, a small section of the grain boundary will suddenly arch toward the side with high dislocation density to form a recrystallization core. This process is also called strain-induced grain boundary migration. This patent adopts a large reduction process during hot rolling, which can produce more grain boundaries, thus having higher deformation energy storage. Under the dominant role of the grain boundary arch nucleation mechanism, more grain boundaries form more nucleation particles. Since there is not enough space for the grains to grow unevenly, more uniform and fine grains are eventually generated, which makes the plate white with high brightness and no heterochromatic stripes after anodizing. However, the conventional pass reduction cannot achieve a good grain refinement effect, and the grain distribution is uneven, and heterochromatic stripes appear on the surface after anodizing, affecting the surface performance of the plate.
[0114] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an anodized 5-series aluminum alloy material, characterized in that: include: Step S1, preparing raw materials: the composition of the anodized 5-series aluminum alloy material includes 0-0.04% Si, 0-0.06% Fe, 1.8%-3.5% Mn, 0.01%-0.04% Ti, and does not contain Cu, and the balance is Al and unavoidable impurity elements. The raw materials are prepared according to the composition of the anodized 5-series aluminum alloy material; Step S2, melting and casting: melting and casting the raw materials in sequence to obtain an ingot; Step S3, hot rolling: hot rolling the ingot for at least 5 times, and the reduction amount of each hot rolling is independently 40 mm to 70 mm, to obtain a hot-rolled material; Step S4, cold rolling: performing multiple cold rolling on the hot rolled material, wherein the multiple cold rolling processes include at least one intermediate annealing, and each intermediate annealing is arranged between two adjacent cold rollings, to obtain a cold rolled material; Step S5, heat treatment of finished product: heat treatment of the cold-rolled material to obtain a heat-treated material; Step S6, surface treatment: performing surface treatment on the heat-treated material, wherein the surface treatment includes anodizing treatment to obtain the anodized 5-series aluminum alloy material.
2. The method for preparing anodized 5-series aluminum alloy material according to claim 1, characterized in that: The number of hot rolling in step S3 is no more than 12 times, and the reduction amount of each hot rolling is independently 60 mm to 70 mm.
3. The method for preparing anodized 5-series aluminum alloy material according to claim 1 or 2, characterized in that: In step S3, the final rolling thickness of the hot rolling is 6 mm to 9 mm; Preferably, the final rolling thickness of the hot rolling is 8 mm to 9 mm.
4. The method for preparing an anodized 5-series aluminum alloy material according to any one of claims 1 to 3, characterized in that: In step S3, the hot rolling start temperature is 475°C to 485°C, and the final rolling temperature is 270°C to 285°C.
5. The method for preparing anodized 5-series aluminum alloy material according to any one of claims 1 to 4, characterized in that: Before the hot rolling in step S3, the ingot obtained in step S2 is kept warm at a temperature of 500°C to 510°C.
6. The method for preparing an anodized 5-series aluminum alloy material according to any one of claims 1 to 5, characterized in that: The total cold rolling rate of the multiple cold rolling processes is 80% to 90%; Preferably, the intermediate annealing is performed when the total cold rolling ratio of the multiple cold rolling processes reaches 55% to 80%.
7. The method for preparing anodized 5-series aluminum alloy material according to claim 6, characterized in that: The multiple cold rolling process includes two intermediate annealings, and when the total cold rolling rate of the multiple cold rolling reaches 55-65%, the first intermediate annealing is performed, and when the total cold rolling rate of the multiple cold rolling reaches 75-80%, the second intermediate annealing is performed.
8. The method for preparing an anodized 5-series aluminum alloy material according to any one of claims 1 to 7, characterized in that: The temperature of each intermediate annealing is independently 300° C. to 360° C., and the holding time is independently 1 h to 3 h.
9. The method for preparing an anodized 5-series aluminum alloy material according to any one of claims 1 to 8, characterized in that: The heat treatment temperature in step S5 is 160° C. to 220° C., and the heat preservation time is 1 h to 3 h.
10. An anodized 5-series aluminum alloy material, characterized in that: The anodized 5-series aluminum alloy material is prepared by the method for preparing the anodized 5-series aluminum alloy material according to any one of claims 1 to 9, and the surface of the anodized 5-series aluminum alloy material has no heterochromatic stripe defects, and the white brightness L value is ≥90.
11. The anodized 5-series aluminum alloy material according to claim 10, characterized in that: The surface grain size of the anodized 5-series aluminum alloy material is 20 to 40 μm, and the cross-sectional grain size of the material is 15 to 30 μm.
12. Use of the anodized 5-series aluminum alloy material according to claim 10 or 11 as a structural material and / or surface material in the fields of computers, communications and consumer electronic products.