6061 aluminum alloy composite plate with good strength and plasticity and preparation method of 6061 aluminum alloy composite plate

By preparing a sandwich-structured aluminum alloy composite plate with an outer solid solution state and an inner cold-rolled state, and utilizing the heterogeneous structure and second phase precipitation, the trade-off between the strength and plasticity of aluminum alloys was solved, and a high-strength and high-plasticity aluminum alloy composite plate was realized.

CN119040775APending Publication Date: 2024-11-29KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158255.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing aluminum alloy processing technology cannot maintain good ductility while improving strength, which makes aluminum alloys prone to plastic instability in the early stage of tensile deformation, affecting their normal use.

Method used

A sandwich structure of 6061 aluminum alloy composite plate with an outer layer of solution-treated 6061 aluminum alloy plate and an inner layer of cold-rolled 6061 aluminum alloy plate was prepared. The heterogeneous structure in the composite plate generates back stress strengthening, and the strength and plasticity are improved through static recovery and second phase precipitation.

Benefits of technology

The strength and plasticity of the aluminum alloy composite plate are improved, with a yield strength of 375MPa, a tensile strength of 415MPa, and a fracture elongation of 14.2%. The aging treatment at a lower temperature reduces grain size changes and retains the strengthening effect of the heterogeneous structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040775A_ABST
    Figure CN119040775A_ABST
Patent Text Reader

Abstract

The invention discloses a 6061 aluminum alloy composite plate with good strength and plasticity and a preparation method of the 6061 aluminum alloy composite plate, and belongs to the technical field of aluminum alloy processing. The method comprises the steps that S1, a 6061 aluminum alloy plate is subjected to solution treatment and then subjected to water quenching, and a solid solution state 6061 aluminum alloy plate is obtained; s2, the solid solution state 6061 aluminum alloy plate in the step S1 is subjected to cold rolling, and a cold-rolled state 6061 aluminum alloy plate is obtained; s3, the solid-solution-state 6061 aluminum alloy plates obtained in the step S1 and the cold-rolled-state 6061 aluminum alloy plates obtained in the step S2 are stacked according to the structure that one cold-rolled-state 6061 aluminum alloy plate is clamped between two solid-solution-state 6061 aluminum alloy plates; s4, the laminated plates stacked in the step S3 are subjected to rolling compounding; and S5, aging treatment is conducted on the composite plate rolled in the step S4, and the 6061 aluminum alloy composite plate is obtained. The aluminum alloy composite plate prepared through the preparation method has high strength, high plasticity and excellent comprehensive mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy processing, and relates to a 6061 aluminum alloy composite plate with good strength and plasticity and a preparation method thereof. Background Art

[0002] Aluminum alloy is one of the most promising lightweight structural materials. Due to its low density and excellent electrical and thermal conductivity, it is widely used in the automotive and aerospace industries. However, with the rapid development of industrial technology, the performance requirements for aluminum alloys are also increasing.

[0003] At present, equal channel angular extrusion, cumulative roll welding, high pressure torsion and multi-axis forging processes are widely used to produce high specific strength aluminum alloys. The principle of the above methods is to improve the strength of metal materials through severe plastic deformation. However, the above methods all need to sacrifice the ductility of aluminum alloys to improve the strength of metal materials. Low ductility aluminum alloys have limited strain hardening ability and are prone to plastic instability (necking) in the early stage of tensile deformation, which affects the normal use of aluminum alloys. Therefore, the trade-off between strength and ductility remains one of the main bottlenecks in the development of advanced structural materials.

[0004] In the aluminum alloy series, the 6xxx series aluminum alloy has medium strength due to the formation of precipitation phase in the matrix after aging. Among them, the 6061 aluminum alloy has excellent processing performance, good corrosion resistance, high toughness and other excellent characteristics. In order to adapt to the rapid development of industrial technology, it is necessary to conduct further in-depth research on the 6061 aluminum alloy to improve its comprehensive performance and make it have better application effect.

[0005] Therefore, it is necessary to provide a 6061 aluminum alloy composite plate with good strength and plasticity and a preparation method thereof, so as to prepare a 6061 aluminum alloy composite plate with excellent performance so that it can better adapt to the application environment of modern industry. Summary of the invention

[0006] In order to overcome the problems in the background technology, the present invention prepares a 6061 aluminum alloy composite plate with a "sandwich structure" in which the outer layer is a solid solution 6061 aluminum alloy plate and the inner layer is a cold-rolled 6061 aluminum alloy plate. The back stress is strengthened by the heterogeneous structure in the composite plate, so that the strength of the composite plate is further improved. At the same time, the static recovery inside the composite plate and the precipitation of the second phase are improved, and finally a 6061 aluminum alloy composite plate with excellent performance is prepared.

[0007] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0008] In one aspect, the present invention provides a method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity, the preparation method comprising the following steps:

[0009] S1: performing a solution treatment on a 6061 aluminum alloy plate, and then performing water quenching to obtain a solid solution state 6061 aluminum alloy plate;

[0010] S2: cold rolling the solid solution state 6061 aluminum alloy plate in step S1 to obtain a cold rolled 6061 aluminum alloy plate;

[0011] S3: stacking the solid solution 6061 aluminum alloy plate obtained in step S1 and the cold rolled 6061 aluminum alloy plate obtained in step S2 in a structure in which one cold rolled 6061 aluminum alloy plate is sandwiched between two solid solution 6061 aluminum alloy plates;

[0012] S4: rolling and laminating the laminated plates stacked in step S3;

[0013] S5: performing aging treatment on the composite plate after rolling in step S4 to obtain a 6061 aluminum alloy composite plate.

[0014] Preferably, in step S1, the solution treatment temperature is 520-540°C, the solution treatment time is 1-4h, and the water quenching is performed at room temperature (10-30°C).

[0015] Preferably, the cold rolling in step S2 is performed at room temperature (10-30° C.).

[0016] Preferably, before stacking in step S3, the aluminum alloy plates are surface treated.

[0017] Preferably, the specific method of surface treatment is: using 600-mesh sandpaper to polish the surface of the aluminum alloy plate, then using anhydrous ethanol to ultrasonically clean the aluminum alloy plate for 5 to 10 minutes, and then blowing the surface of the aluminum alloy plate dry to complete the surface treatment.

[0018] Preferably, in step S4, the rolling temperature is 20-100° C., the holding time is 10-20 min, the roller speed is 200 r / s, and the rolling pressure is 50%.

[0019] Preferably, in step S5, the aging temperature is 120-140° C., and the aging time is 24-32 hours.

[0020] Preferably, the total thickness ratio of the solid solution state 6061 aluminum alloy plate to the cold rolled state 6061 aluminum alloy plate in the 6061 aluminum alloy composite plate is 2:1.

[0021] Another aspect of the present invention provides a 6061 aluminum alloy composite plate, in which the thickness ratio of the solid solution state 6061 aluminum alloy plate to the cold rolled state 6061 aluminum alloy plate is 2:1.

[0022] Beneficial effects of the present invention:

[0023] 1. The present invention prepares a 6061 aluminum alloy composite plate with improved strength and plasticity, wherein the yield strength can reach 375 MPa, the tensile strength can reach 415 MPa, and the elongation at break can reach 14.2%.

[0024] 2. The present invention reduces the change in the grain size of the composite plate by performing aging treatment at a relatively low temperature, thereby retaining the strengthening effect of the heterogeneous structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the rolling and cladding process of the 6061 aluminum alloy clad plate of the present invention.

[0026] Figure 2 This is a metallographic diagram of the finished product of the 6061 aluminum alloy composite plate of the present invention.

[0027] Figure 3 The metallographic images of the 6061 aluminum alloy composite plate of the present invention before and after aging are shown in Figure 1, wherein (a) is the metallographic image before aging, and (b) is the metallographic image after aging.

[0028] Figure 4 The stress-strain curves of the plates prepared in the examples of the present invention and the comparative examples are shown. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with specific embodiments.

[0030] In the examples and comparative examples of the present invention, chemical reagents not specified were all commercially available analytically pure for experiments.

[0031] Example 1

[0032] In this embodiment, a 6061 aluminum alloy composite plate is prepared by the following steps:

[0033] (1): The initial 4mm and 2mm thick 6061 aluminum alloy plates were cut into 30mm×100mm sheets. The cut 6061 aluminum alloy plates were then solution treated at 540℃ for 2h to remove residual stress and allow the second phase to fully dissolve back into the matrix. They were then water quenched at room temperature to obtain solid solution 6061 aluminum alloy plates. Secondly, the surface of the solid solution 6061 aluminum alloy plate was polished with 600-grit sandpaper, and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was dried with a hair dryer for later use.

[0034] (2): At room temperature, a 4 mm thick solid solution 6061 aluminum sheet was rolled to 2 mm to obtain a cold rolled 6061 aluminum sheet. The rolling process was one pass. The surface of the cold rolled 6061 aluminum sheet was then polished and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was blown dry with a hair dryer for later use.

[0035] (3) A laminated plate is formed by stacking solution-state and cold-rolled 6061 aluminum alloy plates in a structure in which one cold-rolled 6061 aluminum alloy plate is sandwiched between two solution-state 6061 aluminum alloy plates. The total thickness of the laminated plate after stacking is about 6 mm.

[0036] (4): Under the condition of 20°C, the laminate was rolled and compounded, the roller speed was 200r / s, the rolling pressure was 50%, and the holding time was 20min, to obtain a 6061 aluminum alloy composite plate with a thickness of about 3mm, wherein the total thickness of the solid solution aluminum alloy plate was about 2mm, the total thickness of the cold rolled aluminum alloy plate was about 1mm, and the rolling process was one pass. The rolled 6061 aluminum alloy composite plate obtained had a yield strength of 365MPa, a tensile strength of 390MPa, and a fracture elongation of 7.5% at room temperature (as shown in Table 1).

[0037] (5): The rolled 6061 aluminum alloy composite plate was aged at 130°C for 28 hours to obtain a finished 6061 aluminum alloy composite plate having a yield strength of 375 MPa, a tensile strength of 420 MPa, and an elongation at break of 14.2% at room temperature (as shown in Table 1).

[0038] The metallographic image of the finished 6061 aluminum alloy composite plate prepared in this embodiment is as follows: Figure 2 As shown, through Figure 2 It can be seen that the inner layer grains have a greater degree of deformation and finer grains, while the outer layer grains have a smaller degree of deformation and coarser grains; the inner layer fine grains can provide strength for the plate, and the outer layer coarse grains can provide plasticity for the plate; at the same time, the grain sizes on both sides of the layer interface are quite different. During deformation, the strain gradient caused by the non-uniform deformation between the coarse grain layer and the fine grain layer will lead to heterogeneous deformation-induced strengthening, which further improves the strength.

[0039] The metallographic image of the 6061 aluminum alloy composite plate prepared in this embodiment before aging treatment is as follows: Figure 3 (a) shows that the metallographic phase diagram after aging treatment is as follows Figure 3 (b) as shown.

[0040] The stress-strain curves of the rolled 6061 aluminum alloy composite plate and the finished composite plate prepared in this embodiment are shown in FIG. Figure 4 shown.

[0041] Example 2

[0042] In this embodiment, a 6061 aluminum alloy composite plate is prepared by the following steps:

[0043] (1): The initial 4mm and 2mm thick 6061 aluminum alloy plates were cut into 30mm×100mm sheets. The cut 6061 aluminum alloy plates were then solution treated at 520℃ for 4h to remove residual stress and allow the second phase to fully dissolve back into the matrix. They were then water quenched at room temperature to obtain solid solution 6061 aluminum alloy plates. Secondly, the surface of the solid solution 6061 aluminum alloy plate was polished with 600-grit sandpaper, and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was blown dry with a hair dryer for use.

[0044] (2): At room temperature, a 4 mm thick solid solution 6061 aluminum sheet was rolled to 2 mm to obtain a cold rolled 6061 aluminum sheet. The rolling process was one pass. The surface of the cold rolled 6061 aluminum sheet was then polished and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was blown dry with a hair dryer for later use.

[0045] (3) A laminated plate is formed by stacking solution-state and cold-rolled 6061 aluminum alloy plates in a structure in which one cold-rolled 6061 aluminum alloy plate is sandwiched between two solution-state 6061 aluminum alloy plates. The total thickness of the laminated plate after stacking is about 6 mm.

[0046] (4): Under the condition of 100°C, the laminate was rolled and composited, the roller speed was 200r / s, the rolling pressure was 50%, the holding time was 10min, and a 6061 aluminum alloy composite plate with a thickness of about 3mm was obtained, wherein the total thickness of the solid solution aluminum alloy plate was about 2mm, the total thickness of the cold rolled aluminum alloy plate was about 1mm, and the rolling process was one pass. A rolled 6061 aluminum alloy composite plate was obtained.

[0047] (5): The rolled 6061 aluminum alloy composite plate was aged at 120°C for 32 hours to obtain a finished 6061 aluminum alloy composite plate having a yield strength of 379 MPa, a tensile strength of 414 MPa, and a fracture elongation of 13.9% at room temperature (as shown in Table 1).

[0048] The stress-strain curves of the rolled 6061 aluminum alloy composite plate and the finished composite plate prepared in this embodiment are shown in FIG. Figure 4 shown.

[0049] Example 3

[0050] In this embodiment, a 6061 aluminum alloy composite plate is prepared by the following steps:

[0051] (1): The initial 4mm and 2mm thick 6061 aluminum alloy plates were cut into 30mm×100mm sheets. The cut 6061 aluminum alloy plates were then solution treated at 530℃ for 1h to remove residual stress and allow the second phase to fully dissolve back into the matrix. They were then water quenched at room temperature to obtain solid solution 6061 aluminum alloy plates. Secondly, the surface of the solid solution 6061 aluminum alloy plate was polished with 600-grit sandpaper, and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was blown dry with a hair dryer for use.

[0052] (2): At room temperature, a 4 mm thick solid solution 6061 aluminum sheet was rolled to 2 mm to obtain a cold rolled 6061 aluminum sheet. The rolling process was one pass. The surface of the cold rolled 6061 aluminum sheet was then polished and then cleaned in an ultrasonic cleaner filled with anhydrous ethanol for 5 to 10 minutes to remove the oxide layer and oil stains on the surface of the sample. Finally, the surface was blown dry with a hair dryer for later use.

[0053] (3) A laminated plate is formed by stacking solution-state and cold-rolled 6061 aluminum alloy plates in a structure in which one cold-rolled 6061 aluminum alloy plate is sandwiched between two solution-state 6061 aluminum alloy plates. The total thickness of the laminated plate after stacking is about 6 mm.

[0054] (4): Under the condition of 60°C, the laminate was rolled and composited, the roller speed was 200r / s, the rolling pressure was 50%, the holding time was 15min, and a 6061 aluminum alloy composite plate with a thickness of about 3mm was obtained, wherein the total thickness of the solid solution aluminum alloy plate was about 2mm, the total thickness of the cold rolled aluminum alloy plate was about 1mm, and the rolling process was one pass. A rolled 6061 aluminum alloy composite plate was obtained.

[0055] (5): The rolled 6061 aluminum alloy composite plate was aged at 140°C for 24 hours to obtain a finished 6061 aluminum alloy composite plate having a yield strength of 370 MPa, a tensile strength of 411 MPa, and a fracture elongation of 14.4% at room temperature (as shown in Table 1).

[0056] The stress-strain curves of the rolled 6061 aluminum alloy composite plate and the finished composite plate prepared in this embodiment are shown in FIG. Figure 4 shown.

[0057] Comparative Example 1

[0058] The aluminum alloy plate is prepared in the same method as in Example 1. The difference is that the aluminum alloy plate in this comparative example is obtained by directly rolling the solid solution plate, and is a non-composite plate. The yield strength of the rolled aluminum alloy plate prepared in this comparative example is 290 MPa, the tensile strength is 308 MPa, and the elongation at break is 9.5% (as shown in Table 1). Its stress-strain curve is as follows: Figure 4 As shown, the 6061 aluminum alloy product prepared in this comparative example has a yield strength of 320 MPa, a tensile strength of 354 MPa, and a fracture elongation of 14.5%. Its stress-strain curve is shown in Figure 4 shown.

[0059] Comparative Example 2

[0060] This comparative example adopts the same method as Example 1 to prepare a 6061 aluminum alloy composite plate, except that: the aluminum alloy composite plate of this comparative example is stacked in a manner that one solid solution state 6061 aluminum alloy plate is sandwiched between two cold-rolled 6061 aluminum alloy plates. The 6061 aluminum alloy product prepared in this comparative example has a yield strength of 382 MPa, a tensile strength of 417 MPa, and an elongation at break of 10.3% (as shown in Table 1).

[0061] Comparative Example 3

[0062] This comparative example adopts the same method as Example 1 to prepare a 6061 aluminum alloy composite plate, except that the aging treatment temperature of this comparative example is 180° C. The 6061 aluminum alloy finished product prepared in this comparative example has a yield strength of 345 MPa, a tensile strength of 369 MPa, and an elongation at break of 11.3% (as shown in Table 1).

[0063] Table 1 Mechanical properties of different aluminum alloy plates

[0064]

[0065] Through Table 1 and Figure 4 It can be seen that compared with the 6061 aluminum alloy composite plate (Rolling) before aging treatment, the strength and elongation at break of the 6061 aluminum alloy composite plate (Age) after aging treatment are improved. This is because the grain size of the 6061 composite plate after rolling is small, and a large number of dislocations remain in its structure during the rolling and compounding process. The number of dislocations that can be accommodated in a grain is certain. In the subsequent stretching process, the dislocations further proliferate and entangle, causing stress concentration in the grain earlier, thereby affecting its elongation. The grain size of the 6061 aluminum alloy composite plate after aging treatment is not much different from that of the 6061 aluminum alloy composite plate before aging treatment (such as Figure 3This shows that although the lower aging temperature cannot provide enough energy for the grain boundary to expand across the barrier, it can reduce the dislocation density in the organization to a certain extent, accompanied by a certain amount of second phase precipitation. Therefore, the 6061 aluminum alloy composite plate after aging treatment shows better mechanical properties.

[0066] By comparing Example 1 with Comparative Example 1, the yield strength and tensile strength of the aluminum alloy composite plate prepared in Example 1 are improved, while the elongation at break remains basically unchanged. This is because the states of the inner and outer layers of the composite plate are different. The different organizational characteristics of the inner and outer layers after rolling cause the plate to produce additional strengthening and work hardening effects, so that the 6061 aluminum alloy composite plate shows excellent comprehensive performance.

[0067] By comparing the embodiment with comparative example 2, it can be seen that although the yield strength and tensile strength of comparative example 2 are slightly improved compared with embodiment 1, the yield strength and tensile strength are only improved by 0.7% relative to embodiment 2, while the elongation at break is reduced by about 26%. It can be seen that the comprehensive performance of the aluminum alloy of comparative example 2 is greatly affected. This is because the strain response rate of the softer coarse-grained layer is faster during deformation, while the strain response rate of the fine-grained layer is slower. In the embodiment, the coarse-grained layer is in the outer layer, and the overall deformation can be coordinated by necking on the outside, while the coarse-grained layer of comparative example 2 is in the inner layer. During deformation, the strains at the interface are incompatible and cannot be coordinated, which will lead to the premature generation of cracks and reduce the elongation at break.

[0068] By comparing the embodiment with comparative example 3, it can be seen that the yield strength, tensile strength and elongation at break of the alloy in comparative example 3 are significantly reduced compared with those in the embodiment, and the comprehensive performance of comparative example 3 is significantly reduced. This is because the aging temperature is too high, a large number of dislocations are dissolved during the aging process, which greatly reduces the effect of work hardening. At the same time, the migration of the precipitated phase and part of the grain boundaries will make the stress in the deformation process of the alloy more easily concentrated, and more prone to fracture.

[0069] In summary, the 6061 aluminum alloy composite plate prepared by the method of the present invention has high strength and high plasticity, and the composite plate has excellent comprehensive mechanical properties.

[0070] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity, Features: The preparation method comprises the following steps: S1: performing a solution treatment on a 6061 aluminum alloy plate, and then performing water quenching to obtain a solid solution state 6061 aluminum alloy plate; S2: cold rolling the solid solution state 6061 aluminum alloy plate in step S1 to obtain a cold rolled 6061 aluminum alloy plate; S3: stacking the solid solution 6061 aluminum alloy plate obtained in step S1 and the cold rolled 6061 aluminum alloy plate obtained in step S2 in a structure in which one cold rolled 6061 aluminum alloy plate is sandwiched between two solid solution 6061 aluminum alloy plates; S4: rolling and laminating the laminated plates stacked in step S3; S5: performing aging treatment on the composite plate after rolling in step S4 to obtain a 6061 aluminum alloy composite plate.

2. A method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 1, Features: In the step S1, the solution treatment temperature is 520-540° C., the solution treatment time is 1-4 hours, and the water quenching is performed at room temperature.

3. The method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 1, Features: The cold rolling in step S2 is performed at room temperature.

4. The method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 1, Features: Before stacking in step S3, the aluminum alloy plates are subjected to surface treatment.

5. A method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 4, Features: The specific method of the surface treatment is: using 600-mesh sandpaper to polish the surface of the aluminum alloy plate, then using anhydrous ethanol to ultrasonically clean the aluminum alloy plate for 5 to 10 minutes, and then blowing the surface of the aluminum alloy plate dry to complete the surface treatment.

6. The method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 1, Features: In step S4, the rolling temperature is 20-100° C., the holding time is 10-20 min, the roller speed is 200 r / s, and the rolling pressure is 50%.

7. The method for preparing a 6061 aluminum alloy composite plate with good strength and plasticity according to claim 1, Features: In the step S5, the aging temperature is 120-140° C., and the aging time is 24-32 hours.

8. The 6061 aluminum alloy composite plate prepared by the preparation method according to any one of claims 1 to 7, Features: The total thickness ratio of the solid solution state 6061 aluminum alloy plate and the cold rolled state 6061 aluminum alloy plate in the 6061 aluminum alloy composite plate is 2:1.