Equipment and method for improving growth quality of multilayer film stack and application of equipment and method

By designing equipment compatible with ALD and PVD processes, integrating growth chambers and multiple excitation devices, the high cost and complex process problems caused by independent equipment in the prior art are solved, and the compatibility of high-purity films and rapid deposition is achieved, and the device is improved Performance and equipment maintenance cycle.

CN119040854APending Publication Date: 2024-11-29KUNSHAN GCL OPTOELECTRONIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411170514.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, atomic layer deposition (ALD) equipment and physical vapor deposition (PVD) equipment exist independently, resulting in high production costs, complex process flow, and short equipment maintenance cycles, which cannot meet the high-purity thin films and rapid deposition in semiconductor devices. simultaneous demand.

Method used

Design a device that is compatible with ALD and PVD processes, integrates growth chamber, environmental regulation unit, precursor supply unit, atomic layer deposition and physical vapor deposition excitation device to achieve the growth of multi-layer film stacks on the same device, combined with ALD and PVD technology performs thin film deposition and is equipped with a by-product treatment system to reduce equipment costs and extend maintenance cycles.

Benefits of technology

It achieves compatibility between high-purity films and rapid deposition on a single device, reduces production costs, simplifies process flow, improves device performance, and extends the maintenance cycle and service life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040854A_ABST
    Figure CN119040854A_ABST
Patent Text Reader

Abstract

The invention discloses equipment and a method for improving the growth quality of a multilayer film stack and application of the equipment and the method. The equipment comprises a growth chamber as well as a first environment adjusting unit, a first precursor supply unit, a second precursor supply unit, an atomic layer deposition excitation device, a physical vapor deposition excitation device and a first conveying device which are matched with the growth chamber, wherein the first environment adjusting unit is used for adjusting the temperature and vacuum degree in the growth chamber; the first precursor supply unit is used for providing a first precursor, and the second precursor supply unit is used for providing a second precursor; the atomic layer deposition excitation device is used for converting the first precursor into an atomic layer deposition layer, and the physical vapor deposition excitation device is used for converting the second precursor into a physical vapor deposition layer. The ALD equipment and the PVD equipment are integrated, the ALD deposition process and the PVD deposition process can be completed in the same chamber at the same time, the growth quality of the multi-layer thin film stack can be improved, and the technological process is simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention particularly relates to a device, a method and an application thereof for improving the growth quality of a multilayer thin film stack, and belongs to the technical field of semiconductor manufacturing equipment. Background Art

[0002] Atomic layer deposition (ALD) is a method of depositing a substance layer by layer on a substrate surface in the form of single atoms. In the ALD process, the chemical reaction of a new layer of atomic film is directly related to the previous layer, so that only one layer of atoms is deposited each time. There are two main reactants of ALD, which are usually called precursors. The precursor reacts continuously and self-limitingly with the surface of the material to achieve the deposition of the thin film. Physical vapor deposition (PVD) is a technology for thin film deposition through physical mechanisms, such as evaporation and sputtering. The PVD process does not involve chemical reactions, so the deposited materials are of high purity and stable quality. Sputtering technology has the advantages of fast deposition rate, accurate deposition thickness control, precise composition control and low manufacturing cost, and is widely used in the semiconductor industry.

[0003] As the performance requirements of semiconductor devices continue to increase, the aspect ratio of the structure in the device continues to increase and the structure becomes more complex. The thin films used in semiconductor materials even need to be controlled in units of atoms. At this time, a better step coverage film layer is needed to act as a buffer layer or a barrier layer. This functional film layer can effectively protect the diffusion and oxidation of the device interface, and can also modify the poor interface to improve the performance of the device; however, the deposition rate of the ALD equipment is very slow and the equipment cost is high, which affects the production efficiency; although the PVD equipment can achieve a higher deposition rate, generally 0.1nm / s~20nm / s, the density of the film layer deposited by PVD is not enough and there is no good step coverage. The new energy cannot meet the application requirements. The current existing technical route is to purchase two types of equipment, namely PVD equipment and ALD equipment, which greatly increases the production cost, and the production efficiency and even the performance of the device are greatly reduced. However, if the integrated equipment of atomic layer deposition and physical vapor deposition can be combined, different types of thin films can be prepared on a single device. This equipment can not only achieve precise control of film thickness, composition and structure during the process preparation, but also meet various application scenarios. For example, in semiconductor device manufacturing, ALD can be used to prepare high-purity ultra-thin film layers, while in the metallization process, PVD technology can be used to achieve fast and accurate thin film deposition.

[0004] In summary, the method of combining atomic layer deposition with physical vapor deposition has a wide range of applications and superior performance, providing strong technical support for the field of thin film preparation.

[0005] In the existing technology, PVD equipment and ALD equipment are independent equipment, and the cost of using the equipment is very high for production enterprises; the process flow is also independent, such as Figure 1 As shown, two independent process flows will make the overall process more complicated, bring inconvenience to production and reduce production efficiency. In the prior art, the by-products generated in the process need to be equipped with multiple sets of additional by-product treatment devices, which further increases the equipment cost; while the present invention reasonably integrates the by-product treatment system into the equipment itself, and adds the required by-product treatment device at a certain position, which can not only reduce the construction cost of the equipment, but also effectively protect the equipment and extend the maintenance cycle of the equipment. Summary of the invention

[0006] The main purpose of the present invention is to provide a device for improving the growth quality of a multilayer thin film stack, thereby overcoming the deficiencies in the prior art.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0008] A first aspect of an embodiment of the present invention provides a device for improving the growth quality of a multilayer thin film stack, comprising:

[0009] A growth chamber, used to provide a closed environment for the growth of a multilayer thin film stack, wherein the growth chamber is provided with a plurality of process windows and a plurality of baffles, each of the baffles matches at least one process window, and the baffles are used to open and close the corresponding process window;

[0010] A first environment adjustment unit, used for adjusting the temperature and vacuum degree in the growth chamber to form an environment required for the growth of a multi-layer thin film stack in the growth chamber;

[0011] A plurality of precursor supply units, each of which is independently connected to the plurality of process windows, and each of which is used to provide a first precursor required for atomic layer deposition or a second precursor required for physical vapor deposition to the growth chamber from the corresponding process window;

[0012] At least one atomic layer deposition excitation device and at least one physical vapor deposition excitation device, the atomic layer deposition excitation device is used to transform the first precursor in the growth chamber into an atomic layer deposition layer, and the physical vapor deposition excitation device is used to transform the second precursor in the growth chamber into a physical vapor deposition layer;

[0013] The conveying device is arranged in the growth chamber and is used for transferring the sample in the growth chamber and driving the sample to move back and forth.

[0014] A second aspect of an embodiment of the present invention provides a method for improving the growth quality of a multilayer thin film stack, the method being implemented by the apparatus for improving the growth quality of a multilayer thin film stack, and the method comprising:

[0015] The temperature and vacuum degree in the growth chamber are adjusted by a first environment adjustment unit to form an environment required for the growth of a multilayer thin film stack in the growth chamber, and at least one first precursor or at least one second precursor is injected into the growth chamber in sequence by a plurality of the precursor supply units respectively, and at least one of the first precursors is converted into at least one atomic layer deposition layer by at least one atomic layer deposition excitation device, and at least one of the second precursors is converted into at least one physical vapor deposition layer by at least one physical vapor deposition excitation device; at least one atomic layer deposition layer and at least one physical vapor deposition layer are stacked in sequence to form a multilayer thin film stack.

[0016] A third aspect of an embodiment of the present invention provides a method for manufacturing a perovskite solar cell, the method being implemented based on the device for improving the growth quality of a multilayer thin film stack, and the method comprising:

[0017] Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the transparent conductive film, injecting a transparent conductive film material precursor into the growth chamber, and converting the transparent conductive film material precursor into a transparent conductive film material by a physical deposition excitation device, thereby forming a transparent conductive film on a substrate;

[0018] The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the hole transport layer, a hole transport layer material precursor is injected into the growth chamber, and the hole transport layer material precursor is converted into a hole transport layer material by a physical deposition excitation device, thereby forming a hole transport layer on the transparent conductive film;

[0019] taking the formed sample out of the growth chamber, and forming a perovskite light absorbing layer on the hole transport layer;

[0020] The sample after forming the perovskite light absorbing layer is transferred into a growth chamber, the temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the electron transport layer, an electron transport layer material precursor is injected into the growth chamber, and the electron transport layer material precursor is converted into an electron transport layer material by a physical deposition excitation device, thereby forming an electron transport layer on the perovskite light absorbing layer;

[0021] Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the buffer layer, injecting a buffer layer material precursor into the growth chamber, and converting the buffer layer material precursor into a buffer layer material by an atomic layer deposition excitation device, thereby forming a buffer layer on the electron transport layer;

[0022] The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the metal electrode, a metal electrode material precursor is injected into the growth chamber, and the metal electrode material precursor is converted into a metal electrode material by an atomic layer deposition excitation device, thereby forming a metal electrode on the buffer layer.

[0023] Compared with the prior art, the advantages of the present invention include:

[0024] An embodiment of the present invention provides a device that is compatible with atomic layer deposition and physical vapor deposition processes, integrating an ALD device with a PVD device, and can simultaneously complete the ALD deposition process and the PVD deposition process in the same chamber, thereby saving equipment costs and simplifying the process flow.

[0025] An embodiment of the present invention provides a device that is compatible with atomic layer deposition and physical vapor deposition processes. The reasonable use of sub-nanometer layers deposited by ALD in combination with film layers deposited by PVD can not only achieve corresponding functions but also effectively further improve the performance of the device.

[0026] An embodiment of the present invention provides a device that is compatible with atomic layer deposition and physical vapor deposition processes and has a reasonable by-product treatment system layout, which can effectively extend the equipment maintenance cycle and protect environmental safety while reducing the equipment construction cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a process flow chart of atomic layer deposition and physical vapor deposition in the prior art;

[0028] Figure 2 It is a partial structural schematic diagram of a device compatible with atomic layer deposition and physical vapor deposition processes provided in a typical implementation case of the present invention;

[0029] Figure 3 It is a schematic diagram of a process flow of an equipment compatible with atomic layer deposition and physical vapor deposition processes provided in a typical implementation case of the present invention;

[0030] Figure 4 It is a schematic diagram of the structure of an inverted pin perovskite solar cell. DETAILED DESCRIPTION

[0031] In view of the deficiencies in the prior art, the inventor of this case, after long-term research and extensive practice, was able to propose the technical solution of the present invention.

[0032] The present invention is particularly important for the PSCs industry. If the product PVSK is exposed to water and oxygen in the air for a long time during the process flow, it will be degraded; in addition, during the process flow, the device will inevitably be polluted by the external environment, and these problems will affect the performance of the device.

[0033] In order to deal with the above problems, the present invention integrates ALD and PVD equipment into one device; in such a device, the two technologies of atomic layer deposition (ALD) and physical vapor deposition (PVD) are combined together to achieve more complex thin film deposition and multi-layer thin film stacking. ALD technology can provide very uniform and dense thin films, while PVD technology has a fast deposition speed and good adhesion. Therefore, the combination of the two can not only overcome their respective limitations and achieve a more optimized thin film deposition effect, but also solve the complex process flow, reduce equipment costs, and optimize device performance. This equipment has broad application prospects in the fields of microelectronics, optoelectronics, nanotechnology, etc.

[0034] A first aspect of an embodiment of the present invention provides a device for improving the growth quality of a multilayer thin film stack, comprising:

[0035] A growth chamber, used to provide a closed environment for the growth of a multilayer thin film stack, wherein the growth chamber is provided with a plurality of process windows and a plurality of baffles, each of the baffles matches at least one process window, and the baffles are used to open and close the corresponding process window;

[0036] A first environment adjustment unit, used for adjusting the temperature and vacuum degree in the growth chamber to form an environment required for the growth of a multi-layer thin film stack in the growth chamber;

[0037] A plurality of precursor supply units, each of which is independently connected to the plurality of process windows, and each of which is used to provide a first precursor required for atomic layer deposition or a second precursor required for physical vapor deposition to the growth chamber from the corresponding process window;

[0038] At least one atomic layer deposition excitation device and at least one physical vapor deposition excitation device, the atomic layer deposition excitation device is used to transform the first precursor in the growth chamber into an atomic layer deposition layer, and the physical vapor deposition excitation device is used to transform the second precursor in the growth chamber into a physical vapor deposition layer;

[0039] The conveying device is arranged in the growth chamber and is used for transferring the sample in the growth chamber and driving the sample to move back and forth.

[0040] Further, the conveying device includes a transmission structure and a motion execution structure, the transmission structure and the motion execution structure are in transmission cooperation, the motion execution structure is used to carry the sample, and an isolation mechanism is further provided in the growth chamber, the motion execution structure is provided on a side of the isolation mechanism close to the process window, and the transmission structure is provided on a side of the isolation mechanism facing away from the process window;

[0041] Furthermore, the device for improving the growth quality of a multilayer thin film stack includes a plurality of atomic layer deposition excitation devices and a plurality of physical vapor deposition excitation devices, and the plurality of atomic layer deposition excitation devices and the plurality of physical vapor deposition excitation devices are arranged in sequence along the conveying direction of a conveying device, and the conveying device is used to transfer samples to working areas corresponding to the plurality of atomic layer deposition excitation devices and the plurality of physical vapor deposition excitation devices in the growth chamber.

[0042] Furthermore, the motion execution structure may include a plurality of rolling bodies that are arranged in sequence along a selected direction and are capable of rotating around their own axes. By driving the plurality of rolling bodies to rotate synchronously in the same direction, the samples located on the plurality of rolling bodies can be moved along the selected direction. The transmission structure includes a plurality of meshing gears or other structures that can realize motion transmission, which are not specifically limited here. The rolling body may be a ball or a roller, etc.

[0043] In a more specific embodiment, the device for improving the growth quality of a multilayer thin film stack further includes: a monitoring unit, the monitoring unit is used to monitor at least one of the deposition rate of the physical vapor deposition layer / the atomic layer deposition layer, the thickness of the physical vapor deposition layer / the atomic layer deposition layer, the temperature in the growth chamber, and the pressure. More specifically, the monitoring unit may include a temperature sensor, an air pressure sensor, a visual monitor, and processing software that cooperates with the visual monitor, etc. The temperature sensor and the air pressure sensor are arranged inside the growth chamber, and the visual monitor can be arranged inside or outside the growth chamber. The structure and composition of the monitoring unit itself and the way in which it realizes the above functions are all known to those skilled in the art and are not specifically limited here. More specifically, the monitoring unit also includes a safety monitoring mechanism, which is used to monitor and alarm information such as gas leakage, temperature exceeding the standard, and vacuum leakage in the growth chamber.

[0044] In a more specific embodiment, the device for improving the growth quality of a multilayer thin film stack further includes: a control unit, the control unit is connected to the monitoring unit, the first environmental adjustment unit, the first precursor supply unit, the second precursor supply unit, the atomic layer deposition excitation device, the physical vapor deposition excitation device, and the first conveying device, and is used to adjust the deposition rate of the physical vapor deposition layer / the atomic layer deposition layer, the temperature and pressure in the growth chamber, and at least one of the supply flow rates of the first precursor and the second precursor. Specifically, the control unit may include a PLC controller and a corresponding control program. It should be noted that the PLC controller and the corresponding control program can be purchased commercially, and their specific structure and working principle will not be described in detail here.

[0045] In a more specific embodiment, the device for improving the growth quality of a multilayer thin film stack also includes: a preheating chamber and a second environmental adjustment unit, wherein the preheating chamber and the growth chamber have two working states: interconnected and isolated from each other, and the second environmental adjustment unit is used to adjust the temperature and vacuum degree in the growth chamber.

[0046] In a more specific embodiment, the apparatus for improving the growth quality of a multilayer thin film stack further comprises: a second conveying device, which is disposed in the preheating chamber and is used to transfer samples in the preheating chamber and to transfer the samples to the first conveying device.

[0047] In a more specific embodiment, the first environmental conditioning unit includes a first heating mechanism and a first vacuum mechanism, the first heating mechanism is integrated in the growth chamber, and the first vacuum mechanism is connected to the growth chamber via a connecting pipe, and the second environmental conditioning unit includes a second heating mechanism and a second vacuum mechanism, the second heating mechanism is integrated in the preheating chamber, and the second vacuum mechanism is connected to the preheating chamber via a connecting pipe, wherein the first vacuum mechanism and the second vacuum mechanism are integrated into one.

[0048] In a more specific embodiment, the device for improving the growth quality of a multilayer thin film stack also includes: a unloading chamber and a third environmental adjustment unit, wherein the unloading chamber and the growth chamber have two working states: interconnected and isolated from each other, and the third environmental adjustment unit is used to adjust the temperature and vacuum degree in the unloading chamber.

[0049] In a more specific embodiment, the apparatus for improving the growth quality of a multilayer thin film stack further comprises: a third conveying device, which is disposed in the unloading chamber and is used to receive samples conveyed by the first conveying device and to transfer samples in the unloading chamber.

[0050] In a more specific embodiment, the third environmental conditioning unit includes a third heating mechanism and a third vacuum mechanism, the third heating mechanism is integrated in the unloading chamber, and the third vacuum mechanism is connected to the unloading chamber via a connecting pipeline, wherein the first vacuum mechanism, the second vacuum mechanism and the third vacuum mechanism are integrated into one.

[0051] In a more specific embodiment, the device for improving the growth quality of a multilayer thin film stack also includes: a by-product processing unit, which is connected to the growth chamber and is used to collect and / or purify the by-products generated in the growth chamber and the remaining first precursor and second precursor.

[0052] Furthermore, the first vacuum pumping mechanism, the second vacuum pumping mechanism and the third vacuum pumping mechanism can be integrated, that is, the same vacuum pumping mechanism is connected to and cooperates with the growth chamber, the preheating chamber and the unloading chamber at the same time, the first vacuum pumping mechanism, the second vacuum pumping mechanism and the third vacuum pumping mechanism can be vacuum pumps, etc., and the first heating mechanism, the second heating mechanism and the third heating mechanism can be electric heating plates or heating wires, etc.

[0053] A second aspect of an embodiment of the present invention provides a method for improving the growth quality of a multilayer thin film stack, the method being implemented by the apparatus for improving the growth quality of a multilayer thin film stack, and the method comprising:

[0054] The temperature and vacuum degree in the growth chamber are adjusted by a first environment adjustment unit to form an environment required for the growth of a multilayer thin film stack in the growth chamber, and at least one first precursor or at least one second precursor is injected into the growth chamber in sequence by a plurality of the precursor supply units respectively, and at least one of the first precursors is converted into at least one atomic layer deposition layer by at least one atomic layer deposition excitation device, and at least one of the second precursors is converted into at least one physical vapor deposition layer by at least one physical vapor deposition excitation device; at least one atomic layer deposition layer and at least one physical vapor deposition layer are stacked in sequence to form a multilayer thin film stack.

[0055] Furthermore, during the process of growing the physical vapor deposition layer and / or the atomic layer deposition layer, the conveying device drives the sample thereon to reciprocate in the working area of ​​the physical deposition excitation device or the atomic layer deposition excitation device.

[0056] A third aspect of an embodiment of the present invention provides a method for manufacturing a perovskite solar cell, the method being implemented based on the device for improving the growth quality of a multilayer thin film stack, and the method comprising:

[0057] Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the transparent conductive film, injecting a transparent conductive film material precursor into the growth chamber, and converting the transparent conductive film material precursor into a transparent conductive film material by a physical deposition excitation device, thereby forming a transparent conductive film on a substrate;

[0058] The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the hole transport layer, a hole transport layer material precursor is injected into the growth chamber, and the hole transport layer material precursor is converted into a hole transport layer material by a physical deposition excitation device, thereby forming a hole transport layer on the transparent conductive film;

[0059] taking the formed sample out of the growth chamber, and forming a perovskite light absorbing layer on the hole transport layer;

[0060] The sample after forming the perovskite light absorbing layer is transferred into a growth chamber, the temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the electron transport layer, an electron transport layer material precursor is injected into the growth chamber, and the electron transport layer material precursor is converted into an electron transport layer material by a physical deposition excitation device, thereby forming an electron transport layer on the perovskite light absorbing layer;

[0061] Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the buffer layer, injecting a buffer layer material precursor into the growth chamber, and converting the buffer layer material precursor into a buffer layer material by an atomic layer deposition excitation device, thereby forming a buffer layer on the electron transport layer;

[0062] The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the metal electrode, a metal electrode material precursor is injected into the growth chamber, and the metal electrode material precursor is converted into a metal electrode material by an atomic layer deposition excitation device, thereby forming a metal electrode on the buffer layer.

[0063] Furthermore, when growing the transparent conductive film, the vacuum pressure in the growth chamber is 3.0E-3 Pa to 3.0E-5 Pa.

[0064] Furthermore, the material of the electron transport layer includes at least one of carbon 60, lithium fluoride, magnesium fluoride, and fullerene derivatives.

[0065] Furthermore, the thickness of the electron transport layer is 20 nm to 30 nm.

[0066] Furthermore, when growing the electron transport layer, the vacuum pressure in the growth chamber is 3.0E-3 Pa to 3.0E-5 Pa.

[0067] Furthermore, the material of the buffer layer includes at least one of tin oxide, zinc oxide, titanium oxide and aluminum oxide.

[0068] Furthermore, the thickness of the buffer layer is 5 nm to 30 nm.

[0069] Furthermore, the deposition rate when growing the buffer layer is / loop~ / cycle.

[0070] Furthermore, the material of the metal electrode includes at least one of gold, silver, aluminum and copper.

[0071] Furthermore, the thickness of the metal electrode is 5nm to 30nm.

[0072] Furthermore, when growing the metal electrode, the vacuum pressure in the growth chamber is 1.0E-4 Pa to 3.0E-5 Pa.

[0073] Furthermore, the method for manufacturing the perovskite solar cell also includes: in the process of growing at least one of the transparent conductive film, the hole transport layer, the electron transport layer, the buffer layer, and the metal electrode, the conveying device drives the sample thereon to reciprocate in the working area of ​​the physical deposition excitation device or the atomic layer deposition excitation device.

[0074] Furthermore, the method for manufacturing the perovskite solar cell also includes: preheating the substrate first, and then transferring the substrate into the growth chamber to grow the perovskite solar cell.

[0075] Furthermore, the temperature of the preheating treatment is 70°C to 150°C.

[0076] The technical solution, its implementation process and principle will be further explained below in conjunction with the accompanying drawings. Unless otherwise specified, the functional mechanisms in the embodiments of the present invention are known to those skilled in the art.

[0077] The device provided by the embodiment of the present invention is compatible with atomic layer deposition (ALD) and physical vapor deposition (PVD) processes and has multiple application scenarios, such as semiconductor manufacturing, nanomaterial synthesis, and optical thin film preparation. The device combines the advantages of atomic layer deposition and physical vapor deposition, and can achieve uniform and controllable deposition of thin films.

[0078] In a typical implementation case, an apparatus compatible with atomic layer deposition and physical vapor deposition processes provided by an embodiment of the present invention mainly includes the following functional units and meets the following requirements:

[0079] Equipment structure: For both PVD evaporation source and ALD source, the bottom-out deposition method can be adopted. The equipment should have a common deposition area for atomic layer deposition and physical vapor deposition; the plasma ionization device is installed upstream of the dust filtration device, so that the solid particles generated by the reaction of excess chemical precursors after ionization can be collected by the dust filtration device, and the dust filtration device is installed at the front end / upstream of the vacuum mechanism and the butterfly valve, so as to maximize the protection of the vacuum mechanism and the butterfly valve; optionally, a preheating chamber and a discharge chamber with independently controlled vacuuming are installed upstream and downstream of the growth chamber, respectively, and are equipped with corresponding functions (hardware) to realize heating, sample transmission and other functions, so as to further improve production efficiency.

[0080] Growth chamber: The growth chamber should have high vacuum, high temperature and constant temperature control functions to meet the requirements of different deposition processes. At the same time, the growth chamber should be equipped with a gas introduction system, temperature control system and pressure control system.

[0081] Isolation unit: Different processes should have good isolation (unit) hardware. For example, the isolation device in the growth chamber can effectively protect the transmission part below the growth chamber and reduce maintenance steps. Multiple baffles are used for atomic layer deposition and physical vapor deposition. The precursor supply lines have good isolation performance for different process methods to prevent cross-contamination of precursors.

[0082] Precursor supply unit: To meet the needs of atomic layer deposition and physical vapor deposition, the equipment should be equipped with two or more precursor supply units. The precursors used in atomic layer deposition are usually metal organic compounds; the precursors used in physical vapor deposition can be metals, alloys, carbides, nitrides, oxides, mixtures, etc.

[0083] Monitoring unit: The equipment should be equipped with a real-time monitoring unit to monitor key parameters in the deposition process, such as deposition rate, film thickness, deposition temperature, chamber pressure, etc. The monitoring unit will feed back these key parameters to the control unit, which can adjust the working parameters of the corresponding functional units in real time according to these parameters to achieve excellent film performance and save and record relevant data.

[0084] Control unit: The equipment should be equipped with a complete control unit to achieve precise control of the atomic layer deposition and physical vapor deposition processes. The control unit should include deposition rate control, temperature control, pressure control, gas flow control, pumping speed control, etc. to ensure the stability and repeatability of the ALD and PVD film deposition process.

[0085] Transfer unit: The equipment should be equipped with a transfer unit to facilitate the switching of actions between atomic layer deposition and physical vapor deposition. The transfer unit should have high precision and high reliability to ensure the continuity and consistency of the deposition process.

[0086] Safety measures: In view of the harmful gases and high temperature environment that may be generated during atomic layer deposition and physical vapor deposition, the equipment should have complete safety measures, such as gas leak detection, temperature over-limit alarm, vacuum leak detection, etc. These functions can be realized by the monitoring unit.

[0087] In a typical implementation case, an embodiment of the present invention provides a device compatible with atomic layer deposition and physical vapor deposition processes, including:

[0088] The preheating chamber 101, the growth chamber 102, and the unloading chamber 103 are connected in sequence. The entrance of the preheating chamber 101 is provided with a first chamber door 1303 that can be opened and closed. The communication port between the preheating chamber 101 and the growth chamber 102 is provided with a second chamber door 1301 that can be opened and closed. The communication port between the growth chamber 102 and the unloading chamber 103 is provided with a third chamber door 1302 that can be opened and closed. The exit of the unloading chamber 103 is provided with a fourth chamber door 1304 that can be opened and closed. A plurality of process windows and a plurality of baffles are arranged on the top, each baffle matches at least one process window, and the baffle is used to open and close the process window. The plurality of process windows include a first process window, a second process window, a third process window, a fourth process window, a fifth process window, a sixth process window, and a seventh process window. The plurality of baffles include a first baffle 601, a second baffle 602, a third baffle 603, a fourth baffle 604, a fifth baffle 605, a sixth baffle 606, and a seventh baffle 607. The seven baffles correspond to the seven windows one by one respectively.

[0089] A second conveyor 401 is provided in the preheating chamber 101, a first conveyor 402 is provided in the growth chamber 102, and a third conveyor 403 is provided in the unloading chamber 103. The second conveyor 401, the first conveyor 402, and the third conveyor 403 cooperate end to end to realize the conveyance / transfer of samples in the preheating chamber 101, the growth chamber 102, and the unloading chamber 103;

[0090] The preheating chamber 101, the growth chamber 102, and the unloading chamber 103 are all provided with heating mechanisms. The preheating chamber 101, the growth chamber 102, and the unloading chamber 103 are also connected to the vacuum pump 1101 via connecting pipelines, respectively. The connecting pipelines include three branch pipelines and one main pipeline. The three branch pipelines are respectively connected to the preheating chamber 101, the growth chamber 102, and the unloading chamber 103. The three branch pipelines are connected to the main pipeline, and the main pipeline is connected to the vacuum pump 1101. A first ball valve 1001 is provided on the branch pipeline between the preheating chamber 101 and the vacuum pump 1101, a second ball valve 1002 is provided on the branch pipeline between the growth chamber 102 and the vacuum pump 1101, and a third ball valve 1003 is provided on the branch pipeline between the unloading chamber 103 and the vacuum pump 1101.

[0091] A plurality of first precursor supply units and a plurality of second precursor supply units, wherein the plurality of first precursor supply units correspond to and are connected to the first process window, the third process window, and the fifth process window, respectively, and the first precursor supply unit is used to provide a first precursor required for atomic layer deposition from the process window corresponding thereto into the growth chamber, and the plurality of second precursor supply units correspond to and are connected to the second process window, the fourth process window, the seventh process window, and the sixth process window, respectively, and the second precursor supply unit is used to provide a second precursor required for physical vapor deposition from the process window corresponding thereto into the growth chamber;

[0092] A first chemical source control device 201, a second chemical source control device 202, a third chemical source control device 203 and a plurality of atomic layer deposition excitation mechanisms, wherein the first chemical source control device 201, the second chemical source control device 202 and the third chemical source control device 203 cooperate with a plurality of first precursor supply units respectively and control the working states and working parameters of the first precursor supply units, and the plurality of atomic layer deposition excitation mechanisms are arranged in the growth chamber 102 and are used to convert the first precursor in the growth chamber into an atomic layer deposition layer;

[0093] The first sputtering power supply 301, the second sputtering power supply 302, the third sputtering power supply 303, and the fourth sputtering power supply 304 correspond to the second process window, the fourth process window, the seventh process window, and the sixth process window respectively. The first sputtering power supply 301, the second sputtering power supply 302, the third sputtering power supply 303, and the fourth sputtering power supply 304 cooperate with the target material to transform the second precursor in the growth chamber into a physical vapor deposition layer.

[0094] It should be noted that Figure 2The device shown in the figure is compatible with atomic layer deposition and physical vapor deposition processes. The monitoring unit and the control unit are not shown. The specific structure of the monitoring unit and the control unit and the structure and method of cooperating with other functional units are all known to those skilled in the art, and will not be described in detail here. Specifically, the monitoring unit is used to monitor at least one of the deposition rate of the physical vapor deposition layer / atomic layer deposition layer, the thickness of the physical vapor deposition layer / atomic layer deposition layer, the temperature in the growth chamber, and the pressure. More specifically, the monitoring unit may include a temperature sensor, an air pressure sensor, a visual monitor, and processing software that cooperates with the visual monitor. The temperature sensor and the air pressure sensor are arranged inside the growth chamber, and the visual monitor can be arranged inside or outside the growth chamber. The structure and composition of the monitoring unit itself and the method of realizing the above functions are all known to those skilled in the art, and will not be specifically limited here. More specifically, the monitoring unit also includes a safety monitoring mechanism, which is used to monitor and alarm information such as gas leakage, temperature exceeding the standard, and vacuum leakage in the growth chamber.

[0095] Of course, the device compatible with atomic layer deposition and physical vapor deposition processes provided by the embodiment of the present invention also includes other functional mechanisms that enable it to achieve atomic layer deposition and physical vapor deposition. These are all known to those skilled in the art and will not be elaborated here.

[0096] Specifically, the vacuum pump (ie, vacuum pumping mechanism) 1101 in the present invention can realize vacuum pumping of the preheating chamber 101 , the growth chamber 102 , and the unloading chamber 103 to adjust the vacuum degree in the preheating chamber 101 , the growth chamber 102 , and the unloading chamber 103 .

[0097] Specifically, the structures of the second conveying device 401, the first conveying device 402, and the third conveying device 403 in the present invention can be the same. The second conveying device 401, the first conveying device 402, and the third conveying device 403 can be a conveyor belt structure, a chain conveying structure, a roller conveying structure, etc. Exemplarily, the first conveying device 402 includes a transmission structure and a motion execution structure, the transmission structure and the motion execution structure are in transmission coordination, the motion execution structure is directly transmitted and coordinated with the sample, and an isolation mechanism 501 is also provided in the growth chamber, the motion execution structure is arranged on the side of the isolation mechanism 501 close to the process window, and the motion execution structure is arranged on the side of the isolation mechanism 501 facing away from the process window. The isolation mechanism 501 can prevent the first precursor and the second precursor from causing corrosion and other damage to the transmission structure, thereby protecting the transmission structure. It should be noted that the isolation mechanism 501 can be a partition with holes, etc., and the balls or rollers contained in the motion execution structure are correspondingly exposed in the openings of the partition.

[0098] For details, please refer to Figure 2, an apparatus compatible with atomic layer deposition and physical vapor deposition processes provided by an embodiment of the present invention also includes a by-product treatment unit, which is connected to the preheating chamber 101, the growth chamber 102, and the unloading chamber 103, and is used to collect and / or purify the by-products generated in the growth chamber 102 and the remaining first precursor and second precursor. Specifically, the by-product treatment unit includes a plasma ionization device 701, a dust filter 801, and an acid-base treatment device 1201. The plasma ionization device 701 and the dust filter 801 are sequentially arranged on the main pipe between the vacuum pump 1101 and the growth chamber 102. A butterfly valve 901 is also arranged on the main pipe between the dust filter 801 and the vacuum pump 1101. The acid-base treatment device 1201 is arranged at the end of the main pipe.

[0099] Please also read Figure 3 and Figure 4 The process of preparing an inverted structure pin perovskite solar cell using a compatible atomic layer deposition and physical vapor deposition device includes the following steps:

[0100] 1) A transparent conductive substrate 1 and a hole transport layer (HTL) are prepared on a substrate. The material of the transparent conductive substrate may be indium tin oxide (ITO), aluminum zinc oxide (AZO) or other mixed materials. In this example, the material of the transparent conductive substrate is TCO; the material of the hole transport layer may be copper oxide, nickel oxide, 2,2″,7,7″-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9′-spirobifluorene (Spiro-OMeTAD) or at least one of the following materials.

[0101] In this example, a layer of nickel oxide NiO is deposited as a hole transport layer using the device of the present invention, specifically comprising:

[0102] First, the sample enters the preheating chamber 101 through the second conveying device 401, the second ball valve 1002 and the third ball valve 1003 are closed, the first chamber door 1303 is closed, and the first ball valve 1001 is opened. The preheating chamber 101 is evacuated and the substrate is preheated. The temperature of the preheating chamber 101 and the growth chamber 102 is 70° C. to 150° C. After the preheating is completed, the second chamber door 1301 is opened, and the second chamber door 1301 is closed after the sample enters the growth chamber 102;

[0103] After the first baffle 601, the third baffle 603, the fifth baffle 605, the sixth baffle 606, and the seventh baffle 607 are closed, the plasma ionization device 701 and the acid-base treatment device 1201 are turned on;

[0104] Then, the vacuum pressure in the growth chamber 102 is kept at 3.0E-3 Pa to 3.0E-5 Pa by controlling the butterfly valve 901, the second baffle 602 is opened, and after waiting for a few seconds, the first sputtering power source 301 is turned on to perform the PVD deposition process of the transparent conductive substrate (TCO) 1, and the thickness of the transparent conductive substrate 1 is controlled to be 200 nm to 300 nm;

[0105] After the transparent conductive substrate 1 is deposited, wait for a few seconds, turn off the first sputtering power supply 301, and close the second baffle 602; open the fourth baffle (target baffle) 604, turn on the second sputtering power supply 302, and start the PVD deposition process of the nickel oxide layer, using the nickel oxide layer as the hole transport layer (HTL) 2. After the deposition is completed, turn off the second sputtering power supply 302, close the fourth baffle 604, wait for a certain period of time, turn off the plasma ionization device 701, turn off the acid-base treatment system 1201, close the second ball valve 1002, open the third ball valve 1003 for vacuuming, wait for the vacuum degree of the growth chamber 102 and the unloading chamber 103 to be close, open the third chamber door 1302, and transfer the sample on which the transparent conductive substrate 1 and the hole transport layer (HTL) 2 are deposited to the unloading chamber 103 through the first conveying device 402 and the third conveying device 403, close the third ball valve 1003, close the third chamber door 1302, open the fourth chamber door 1304, and cool the sample to wait for removal.

[0106] 2) A perovskite light absorbing layer (PVSK) 3 is prepared on the hole transport layer (HTL) 2 by using at least one of a spin coating process, a coating process, and a screen printing process. The thickness of the perovskite light absorbing layer (PVSK) 3 is 500 nm.

[0107] 3) depositing an electron transport layer (ETL) 4-1 on the perovskite light absorbing layer (PVSK) 3, wherein the material of the electron transport layer (ETL) 4-1 may be at least one of carbon 60 (C60), lithium fluoride, magnesium fluoride, and fullerene derivatives (PCBM).

[0108] The present invention takes magnesium fluoride (MgF) as an example, and deposits magnesium fluoride (MgF) on the perovskite light absorption layer (PVSK) 3 using the atomic layer deposition and physical vapor deposition equipment compatible with the present invention to form an electron transport layer (ETL) 4-1.

[0109] First, open the first chamber door 1303, send the sample into the preheating chamber 101 through the second conveying device 401, close the second ball valve 1002 and the third ball valve 1003, open the first ball valve 1001, evacuate and preheat the preheating chamber 101, and the temperature of the preheating chamber 101 and the growth chamber 102 is 70°C to 150°C. After the preheating is completed, open the second chamber door 1301, close the second chamber door 1301 and the first ball valve 1001 after the sample enters the growth chamber 102, and open the second ball valve 1002. Confirm that the first baffle 601, the third baffle 603, the fifth baffle 605, and the third baffle 606 are in a state of being fully closed. After the sixth baffle 606 and the seventh baffle 607 are closed; the plasma ionization device 701 and the acid-base treatment device 1201 are turned on; then the vacuum pressure in the growth chamber 102 is kept at 3.0E-3 Pa to 3.0E-5 Pa by controlling the butterfly valve 901, the seventh baffle 607 is opened, and after waiting for a few seconds, the third sputtering power supply 303 is turned on to perform the PVD deposition process of MgF, and the thickness of MgF is controlled to be 20nm to 30nm to form an electron transport layer 4-1; after the electron transport layer 4-1 is deposited, wait for a few seconds, turn off the third sputtering power supply 303, and close the seventh baffle 607.

[0110] 4) Next, a buffer layer 4-2 is prepared by using the atomic layer deposition and physical vapor deposition equipment compatible with the present invention to deposit the buffer layer 4-2 on the electron transport layer 4-1. The material of the buffer layer 4-2 can be selected from at least one of tin oxide, zinc oxide, titanium oxide, and aluminum oxide.

[0111] The present invention takes tin oxide (SnO2) as an example; first, the vacuum value in the growth chamber 102 is adjusted by the butterfly valve 901, and after the vacuum degree reaches 100 Pa to 300 Pa and the pressure is stable, the first baffle 601, the third baffle 603, and the fifth baffle 605 are opened, and the valve on the pipeline of the precursor supply unit is opened through the first chemical source control device 201, the second chemical source control device 202, and the second chemical source control device 203, and the chemical source is introduced into the growth chamber to perform the ALD SnO2 deposition process. During the process, the sample is swung back and forth by the first conveying device 402 during the ALD process deposition to obtain a more uniform film layer, thereby improving the film layer quality. The thickness of SnO2 is 5nm to 30nm, and the deposition rate is controlled at / loop~ / between cycles; after the ALD process deposition is completed, the valve on the pipeline of the precursor supply unit is opened through the first chemical source control device 201, the second chemical source control device 202, and the second chemical source control device 203, the chemical source supply is stopped, and the first baffle 601, the third baffle 603, and the fifth baffle 605 are closed.

[0112] 5) Next, a metal electrode 5 is prepared on the buffer layer 4 - 2 by using a PVD process. The material of the metal electrode 5 can be at least one of gold, silver, aluminum and copper.

[0113] The present invention selects silver (Ag) material as an example; the sample is adjusted to a suitable position by the first conveying device 402, and the vacuum pressure in the growth chamber 102 is stabilized at 1.0E-4 Pa to 3.0E-5 Pa by controlling the butterfly valve 901, and then the sixth baffle 606 is opened, and after waiting for a few seconds, the fourth sputtering power supply 304 is turned on, and Ag with a thickness of 5nm to 30nm is deposited by a PVD process as an electrode layer. After the deposition of the electrode layer is completed, wait for a few seconds, turn off the fourth sputtering power supply 304, close the sixth baffle 606, wait for a certain period of time, turn off the plasma ionization device 701, and turn off the acid-base treatment device 1201; open the third chamber door 1302, and convey the sample to the unloading chamber 103 by the first conveying device 402, close the third chamber door 1302, and after the sample is cooled, open the fourth chamber door 1304 to vent and take it out, and finally make a complete perovskite solar cell (PSCs) device.

[0114] In all of the above process, whether it is ALD or PVD process, as long as the film layer is deposited, by-products will be generated. The by-product treatment unit in the present invention can achieve a better treatment effect on the by-products, which can not only extend the maintenance cycle of the equipment, especially the protection of the pump group and the environment, but also, for example, the plasma treatment device 701 can ionize the by-products in the form of gas that are difficult to treat by conventional methods and then enter the acid-base treatment device 1201 for further inactivation treatment; and the dust filter 801 can collect the solid dust particles generated in the process, reduce the impact of dust particles on the pump group and extend the service life; the acid-base treatment device can effectively treat the waste gas that may be generated in the process, such as hydrogen chloride gas, ammonia gas, etc., and neutralize them in the acid-base treatment device.

[0115] Through the above design, this equipment that is compatible with atomic layer deposition and physical vapor deposition processes can not only achieve uniform and controllable deposition of multiple materials in the same chamber, but also simplify the preparation process of the film layer, providing strong support for research and application in fields such as semiconductors, nanomaterials and optics.

[0116] An embodiment of the present invention provides a device that is compatible with atomic layer deposition and physical vapor deposition processes, which can reduce the cost of equipment use, simplify the process flow and improve production efficiency. The combination of ALD ultra-thin film layer and ideal step coverage with PVD's faster deposition speed and process diversification can overcome their respective limitations and improve device performance.

[0117] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A device for improving the growth quality of a multilayer thin film stack, characterized in that: include: A growth chamber, used to provide a closed environment for the growth of a multilayer thin film stack, wherein the growth chamber is provided with a plurality of process windows and a plurality of baffles, each of the baffles matches at least one process window, and the baffles are used to open and close the corresponding process window; A first environment adjustment unit, used for adjusting the temperature and vacuum degree in the growth chamber to form an environment required for the growth of a multi-layer thin film stack in the growth chamber; A plurality of precursor supply units, each of which is independently connected to the plurality of process windows, and each of which is used to provide a first precursor required for atomic layer deposition or a second precursor required for physical vapor deposition to the growth chamber from the corresponding process window; At least one atomic layer deposition excitation device and at least one physical vapor deposition excitation device, the atomic layer deposition excitation device is used to transform the first precursor in the growth chamber into an atomic layer deposition layer, and the physical vapor deposition excitation device is used to transform the second precursor in the growth chamber into a physical vapor deposition layer; The conveying device is arranged in the growth chamber and is used for transferring the sample in the growth chamber and driving the sample to move back and forth.

2. The device for improving the growth quality of a multilayer thin film stack according to claim 1, characterized in that: The conveying device comprises a transmission structure and a motion execution structure, the transmission structure and the motion execution structure are in transmission cooperation, the motion execution structure is used to carry the sample, and an isolation mechanism is further provided in the growth chamber, the motion execution structure is provided on a side of the isolation mechanism close to the process window, and the transmission structure is provided on a side of the isolation mechanism facing away from the process window; And / or, the equipment for improving the growth quality of a multilayer thin film stack comprises a plurality of atomic layer deposition excitation devices and a plurality of physical vapor deposition excitation devices, wherein the plurality of atomic layer deposition excitation devices and the plurality of physical vapor deposition excitation devices are arranged in sequence along a conveying direction of a conveying device, and the conveying device is used to transfer samples to working areas corresponding to the plurality of atomic layer deposition excitation devices and the plurality of physical vapor deposition excitation devices in the growth chamber.

3. The device for improving the growth quality of a multilayer thin film stack according to claim 1, characterized in that: Also includes: A monitoring unit is used to monitor at least one of the deposition rate of the physical vapor deposition layer / the atomic layer deposition layer, the thickness of the physical vapor deposition layer / the atomic layer deposition layer, the temperature in the growth chamber, and the pressure.

4. The device for improving the growth quality of a multilayer thin film stack according to claim 3, characterized in that: Also includes: A control unit, which is connected to the monitoring unit, the first environmental adjustment unit, the first precursor supply unit, the second precursor supply unit, the atomic layer deposition excitation device, the physical vapor deposition excitation device, and the first conveying device, and is used to adjust the deposition rate of the physical vapor deposition layer / the atomic layer deposition layer, the temperature and pressure in the growth chamber, and at least one of the supply flow rates of the first precursor and the second precursor.

5. The device for improving the growth quality of a multilayer thin film stack according to claim 1, characterized in that: Also includes: A preheating chamber and a second environment adjustment unit, wherein the preheating chamber and the growth chamber have two working states: interconnected and isolated from each other, and the second environment adjustment unit is used to adjust the temperature and vacuum degree in the growth chamber; Preferably, the first environment conditioning unit comprises a first heating mechanism and a first vacuuming mechanism, the first heating mechanism is integrated in the growth chamber, and the first vacuuming mechanism is connected to the growth chamber via a connecting pipeline, and the second environment conditioning unit comprises a second heating mechanism and a second vacuuming mechanism, the second heating mechanism is integrated in the preheating chamber, and the second vacuuming mechanism is connected to the preheating chamber via a connecting pipeline; Preferably, the first vacuum pumping mechanism and the second vacuum pumping mechanism are integrated into one.

6. The device for improving the growth quality of a multilayer thin film stack according to claim 1 or 5, characterized in that: Also includes: A discharge chamber and a third environment adjustment unit, wherein the discharge chamber and the growth chamber have two working states: interconnected and isolated from each other, and the third environment adjustment unit is used to adjust the temperature and vacuum degree in the discharge chamber; Preferably, the third environment adjustment unit comprises a third heating mechanism and a third vacuum pumping mechanism, the third heating mechanism is integrated in the unloading chamber, and the third vacuum pumping mechanism is connected to the unloading chamber via a connecting pipeline; Preferably, the first vacuum pumping mechanism, the second vacuum pumping mechanism and the third vacuum pumping mechanism are integrated into one.

7. A method for improving the growth quality of a multilayer thin film stack, characterized in that: The method is implemented by the device for improving the growth quality of a multilayer thin film stack according to any one of claims 1 to 6, and the method comprises: The temperature and vacuum degree in the growth chamber are adjusted by a first environment adjustment unit to form an environment required for the growth of a multi-layer thin film stack in the growth chamber, at least one first precursor or at least one second precursor is injected into the growth chamber in sequence by a plurality of the precursor supply units, at least one of the first precursors is converted into at least one atomic layer deposition layer by at least one atomic layer deposition excitation device, and at least one of the second precursors is converted into at least one physical vapor deposition layer by at least one physical vapor deposition excitation device; at least one atomic layer deposition layer and at least one physical vapor deposition layer are sequentially stacked to form a multi-layer thin film stack; Preferably, during the process of growing the physical vapor deposition layer and / or the atomic layer deposition layer, the conveying device drives the sample thereon to reciprocate in the working area of ​​the physical deposition excitation device or the atomic layer deposition excitation device.

8. A method for manufacturing a perovskite solar cell, characterized in that: The manufacturing method is implemented by the device for improving the growth quality of a multilayer thin film stack according to any one of claims 1 to 6, and the manufacturing method comprises: Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the transparent conductive film, injecting a transparent conductive film material precursor into the growth chamber, and converting the transparent conductive film material precursor into a transparent conductive film material by a physical deposition excitation device, thereby forming a transparent conductive film on a substrate; The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the hole transport layer, a hole transport layer material precursor is injected into the growth chamber, and the hole transport layer material precursor is converted into a hole transport layer material by a physical deposition excitation device, thereby forming a hole transport layer on the transparent conductive film; taking the formed sample out of the growth chamber, and forming a perovskite light absorbing layer on the hole transport layer; The sample after forming the perovskite light absorbing layer is transferred into a growth chamber, the temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the electron transport layer, an electron transport layer material precursor is injected into the growth chamber, and the electron transport layer material precursor is converted into an electron transport layer material by a physical deposition excitation device, thereby forming an electron transport layer on the perovskite light absorbing layer; Adjusting the temperature and pressure in the growth chamber to the temperature and pressure required for growing the buffer layer, injecting a buffer layer material precursor into the growth chamber, and converting the buffer layer material precursor into a buffer layer material by an atomic layer deposition excitation device, thereby forming a buffer layer on the electron transport layer; The temperature and pressure in the growth chamber are adjusted to the temperature and pressure required for growing the metal electrode, a metal electrode material precursor is injected into the growth chamber, and the metal electrode material precursor is converted into a metal electrode material by an atomic layer deposition excitation device, thereby forming a metal electrode on the buffer layer.

9. The method for manufacturing a perovskite solar cell according to claim 8, characterized in that: When growing the transparent conductive film, the vacuum pressure in the growth chamber is 3.0E-3 Pa to 3.0E-5 Pa; Preferably, the material of the electron transport layer includes at least one of carbon 60, lithium fluoride, magnesium fluoride, and fullerene derivatives; Preferably, the thickness of the electron transport layer is 20 nm to 30 nm; Preferably, when growing the electron transport layer, the vacuum pressure in the growth chamber is 3.0E-3 Pa to 3.0E-5 Pa; Preferably, the material of the buffer layer includes at least one of tin oxide, zinc oxide, titanium oxide and aluminum oxide; Preferably, the thickness of the buffer layer is 5nm to 30nm; Preferably, the deposition rate when growing the buffer layer is Cycle cycle; Preferably, the material of the metal electrode includes at least one of gold, silver, aluminum and copper; Preferably, the thickness of the metal electrode is 5nm to 30nm; Preferably, when growing the metal electrode, the vacuum pressure in the growth chamber is 1.0E-4 Pa to 3.0E-5 Pa.

10. The method for manufacturing a perovskite solar cell according to claim 8 or 9, characterized in that: Also includes: During the process of growing at least one of a transparent conductive film, a hole transport layer, an electron transport layer, a buffer layer, and a metal electrode, the conveying device drives the sample thereon to reciprocate in the working area of ​​a physical deposition excitation device or an atomic layer deposition excitation device. Preferably, the method for manufacturing the perovskite solar cell further comprises: preheating the substrate first, and then transferring the substrate into the growth chamber to grow the perovskite solar cell; Preferably, the temperature of the preheat treatment is 70°C to 150°C.