Gear composite coating for power equipment and preparation method of gear composite coating

By forming a composite coating of zinc-nickel alloy layer and zinc-nickel-phosphorus amorphous alloy layer on the surface of gears in power equipment, the problems of insufficient hardness and corrosion resistance of gear coatings in the prior art are solved, achieving the effects of high hardness, high wear resistance and low cost.

CN119040888APending Publication Date: 2024-11-29STATE GRID HUNAN ELECTRIC POWER COMPANY LIMITED +3
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411153807.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing coatings on gears used in power equipment are insufficient to meet the operational requirements of high-voltage power supply in terms of corrosion resistance, hardness, and cost. In particular, zinc coatings are thin and have low hardness, while electroless nickel-phosphorus alloy coatings have high porosity and high cost.

Method used

A zinc-nickel alloy layer and a zinc-nickel-phosphorus amorphous alloy layer are sequentially formed on the gear surface. The zinc-nickel alloy layer is electroplated, and the zinc-nickel-phosphorus amorphous alloy layer is chemically plated. The thickness and composition of both are optimized to improve hardness and corrosion resistance. Heat treatment and passivation treatment are combined to enhance the performance of the composite coating.

Benefits of technology

The resulting composite coating has a hardness exceeding HV500, corrosion resistance more than 10 times that of electroplated zinc coating, and corrosion resistance more than 3 times that of electroplated zinc coating. It showed no corrosion after 1500 hours of neutral salt spray testing, thus reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040888A_ABST
    Figure CN119040888A_ABST
Patent Text Reader

Abstract

The invention discloses a gear composite coating for electrical equipment and a preparation method of the gear composite coating, the gear composite coating comprises a zinc-nickel alloy layer and a zinc-nickel-phosphorus amorphous alloy layer which are sequentially plated on the surface of a gear, the thickness of the zinc-nickel alloy layer is 5-15 microns, and the thickness of the zinc-nickel-phosphorus amorphous alloy layer is 10-20 microns. The preparation method comprises the following steps that firstly, surface cleaning and activation are conducted on the gear, the zinc-nickel alloy layer is electroplated on the surface of the gear, catalytic activity is generated, then the zinc-nickel-phosphorus amorphous alloy layer is chemically plated, and then heat treatment and passivation treatment are conducted. The formed composite coating has good hardness, wear resistance and corrosion resistance, and the technical problems that in the prior art, a gear surface zinc plating or blackening technology is insufficient in corrosion resistance and hardness and prone to damage, and a zinc-nickel-phosphorus amorphous alloy layer is difficult to be plated on the gear surface thickly and still insufficient in corrosion resistance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrical equipment and electrical engineering, and in particular to a gear composite coating for electric equipment and a preparation method thereof. Background Art

[0002] Transformers, circuit breakers, disconnectors and other power equipment in the power system must be equipped with operating mechanisms. By controlling the operation of the operating mechanisms of the low-voltage circuit part, the connecting rods, crank arms and other transmission parts are used to transmit force or torque to the conductive rods, contacts and other operating parts in the high-voltage circuit to perform operations such as separation, connection and switching. Figure 1 As shown, it includes a mechanism box 14, an internal transmission gear 13 and an electric or hydraulic mechanism 15 located in the mechanism box 14, a transmission crank arm 12 located outside the mechanism box 14, and an external transmission gear 11 passing through the inside and outside of the mechanism box 14, the external transmission gear 11 is connected to the transmission crank arm 12 and the internal transmission gear 13 respectively, and the electric or hydraulic mechanism 15 drives the internal transmission gear 13 to move, so as to realize the separation and operation of the strong power side to control the operation of the power grid, and to separate the high-voltage and low-voltage circuits to ensure the safety of the operator. Transmission gears are used in the operating mechanism to transmit the operating force and torque of the electric or hydraulic mechanism, and adjust the speed or torque. Since the size of the high-voltage and strong power side action parts is large and requires a large operating force, the gears are subjected to large mechanical loads and impact loads at the moment of separation and closing during operation; at the same time, the gears may be infiltrated by moisture in the mechanism box, and some gears may be exposed outside the mechanism box, facing the problem of corrosion. Compared with gears in other industries, which can be completely enclosed indoors or inside equipment and do not require high corrosion resistance, gears used in power equipment require high corrosion resistance because they need to separate strong and weak electricity and run inside and outside the mechanism box 14 at the same time. Neutral salt spray resistance generally needs to reach more than 720 hours. In addition, the instantaneous impact load of opening and closing operations is relatively high, requiring high hardness and wear resistance, otherwise the surface coating will be easily damaged and lose its protective performance.

[0003] In order to meet this operating condition, the gear body is usually made of steel material and electroplated with zinc or chemically oxidized to blacken for corrosion protection. However, there are two major problems with electroplated zinc or black oxide film. First, the coating thickness is relatively thin, usually not exceeding 15 microns, and the anti-corrosion performance is limited. Rust often occurs, especially the exposed gears may be severely rusted in two or three years, resulting in transmission jamming, poor fit, brittle steel parts, and reduced mechanical properties. Second, the teeth on the gears frequently rub and bear impact loads, and the stress concentration at the contact point between teeth is relatively large. The hardness of electroplated zinc and oxide film is relatively low, usually less than 55HV, which is very easy to be partially damaged and contact fatigue occurs. Fatigue cracks occur on the surface, resulting in broken teeth or even gear breakage. Accidents of rust and cracking of gear components, especially ratchets, are common during the operation of power equipment, affecting the safety of the power grid.

[0004] Solving this problem requires a coating with high hardness, high wear resistance and good corrosion resistance, but a single coating is difficult to meet the requirements. Zinc-nickel alloy coatings have good corrosion resistance, which can be more than twice that of electroplated zinc, and are anodic coatings with lower electrode potential than the steel substrate. Even if the coating is partially damaged, it can still play a cathodic protection role to prevent internal steel corrosion, but its hardness is about 200HV, which is still difficult to meet the wear resistance requirements of gear operation. The coating with good wear resistance is chemical nickel-phosphorus alloy coating, which has a high hardness of up to 500HV, but the coating contains phosphorus and has a high porosity. The corrosion resistance and density are not as good as zinc-based alloy coatings. The presence of phosphides increases the corrosion potential. For steel, it is a cathodic protection layer. When there is local damage, the electrochemical protection effect is poor and the substrate is prone to corrosion. In addition, if a nickel-phosphorus alloy coating is directly electroplated on the gear surface, the electroplating requires that the substrate surface has catalytic activity. The gear steel surface has no catalytic activity and is difficult to plate directly. Even if a catalyst is introduced, the deposition rate of the electroplating is slow, the thickness is difficult to meet the requirements of high wear resistance and corrosion resistance, and the cost increases rapidly. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a composite coating for gears of power equipment which is corrosion-resistant, has high hardness and low cost, and a preparation method thereof.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A composite coating for gears of electric power equipment comprises a zinc-nickel alloy layer and a zinc-nickel-phosphorus amorphous alloy layer plated in sequence on the surface of the gear, wherein the zinc-nickel alloy layer has a thickness of 5 to 15 microns, and the zinc-nickel-phosphorus amorphous alloy layer has a thickness of 10 to 20 microns, the zinc-nickel alloy layer is an electroplated layer, and the zinc-nickel-phosphorus amorphous alloy layer is a chemically plated layer.

[0008] As a further improvement of the above technical solution:

[0009] The mass fraction of nickel in the zinc-nickel alloy layer is 5% to 15%, and the rest is zinc; the mass fraction of zinc in the zinc-nickel-phosphorus amorphous alloy layer is 5% to 15%, the mass fraction of phosphorus is 7% to 14%, and the rest is nickel.

[0010] As a general inventive concept, the present invention also provides a method for preparing a composite coating of a gear for electric power equipment, comprising the following steps:

[0011] A1. Remove impurities from the gear surface and perform activation treatment;

[0012] A2. Use the gear as cathode and immerse it in zinc-nickel plating solution with the anode for electroplating to form a zinc-nickel alloy layer on the gear surface and clean the gear;

[0013] A3, immersing the gear in a zinc-nickel-phosphorus plating solution for chemical plating to form a zinc-nickel-phosphorus amorphous alloy layer on the zinc-nickel alloy layer, and cleaning the gear;

[0014] A4. After heat treatment, the gear is immersed in a passivation solution for passivation treatment to obtain a composite coating for gears for power equipment.

[0015] As a further improvement of the above technical solution:

[0016] In step A2, the raw materials of the zinc-nickel plating solution include the following components: ZnO 8-15 g / L, NiSO4·6H2O 10-20 g / L, NaOH 80-150 g / L, sodium citrate 20-60 g / L, triethanolamine 20-60 g / L, vanillin 0.1-0.2 g / L, and the rest is deionized water or distilled water.

[0017] In step A2, during the electroplating process, the current density is 1 to 5 A / dm 2 , time 20 to 40 minutes.

[0018] In step A3, the raw materials of the zinc-nickel-phosphorus plating solution include the following components: ZnSO4·7H2O 2-15 g / L, NiSO4·7H2O 27-35 g / L, NaH2PO2·H2O 10 g / L, sodium citrate 80-90 g / L, NH4Cl 50 g / L, 25% NH4OH solution 60 mL, and the rest is deionized water or distilled water, and the pH value of the zinc-nickel-phosphorus plating solution is 8.2-9.2.

[0019] Preferably, in step A3, the pH value of the zinc-nickel-phosphorus plating solution is controlled to be 8.2-9.2 by using ammonia water.

[0020] In step A3, during the chemical plating treatment, the temperature is 90-100° C. and the time is 20 min-2 h.

[0021] In step A4, the heat treatment temperature is 200-350° C., and the time is 1-3 hours; the passivation solution is a chromate or chromium-free passivation agent solution, and the passivation treatment time is 1-15 minutes.

[0022] In step A1, the impurities include pollutants, oxides and oil.

[0023] In step A1, removing impure oil includes the following steps: immersing the gear in an alkaline bath at 70 to 80° C. for 1 to 10 minutes;

[0024] The raw materials of the alkaline bath liquid include the following components: NaOH 7.5-15 g / L, Na2CO3 35-45 g / L, Na3PO4·12H2O 15-30 g / L, non-ionic surfactant 7.5 g / L, and the rest is deionized water or distilled water.

[0025] In step A1, the gear is immersed in a hydrochloric acid solution for activation treatment, and then washed with deionized water or distilled water.

[0026] Compared with the prior art, the advantages of the present invention are:

[0027] The composite coating for gears of the present invention is a composite coating formed on the surface of the gears, wherein the inner layer is a zinc-nickel alloy layer with a thickness of about 5 to 15 microns, and the outer layer is a zinc-nickel-phosphorus amorphous alloy layer with a thickness of 10 to 20 microns. The inner and outer layers have good compatibility and complementarity. The formed composite coating has good hardness, wear resistance (the higher the hardness, the greater the wear resistance) and corrosion resistance. The surface hardness exceeds HV500, which can be more than 10 times that of the electroplated zinc layer, and the corrosion resistance can also be more than 3 times that of the electroplated zinc layer. There is still no corrosion in neutral salt spray for 1500 hours. At the same time, due to the presence of the zinc-nickel alloy layer, good toughness is maintained, and the production speed is accelerated, the use of expensive nickel is saved, and the total cost is reduced.

[0028] The invention discloses a preparation method of a composite coating of gears for electric power equipment. The method comprises the following steps: firstly electroplating a zinc-nickel alloy layer and introducing a catalyst nickel to generate catalytic activity, so that the catalytic activity of the gears reaches chemical plating conditions, and then generating a highly wear-resistant zinc-nickel-phosphorus amorphous alloy layer. The zinc-nickel plating solution and the zinc-nickel-phosphorus plating solution have similar compositions, thus solving the compatibility problem of the composite plating process. The addition of zinc to the zinc-nickel-phosphorus amorphous alloy layer improves the compatibility with the zinc-nickel alloy layer and the electrochemical protection. In addition, the zinc-nickel-phosphorus amorphous alloy particles in the outer layer can also enter the pores of the zinc-nickel alloy layer to play a sealing role, thereby further improving the corrosion resistance of the composite coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the operating mechanism for the electric power equipment of the present invention.

[0030] Figure 2 Schematic diagram of the gear plating structure of the present invention.

[0031] Figure 3 It is a flow chart of the preparation method of the present invention.

[0032] The symbols in the figure represent:

[0033] 1. Gear; 2. Zinc-nickel alloy layer; 3. Zinc-nickel-phosphorus amorphous alloy layer; 11. External transmission gear; 12. Transmission crank arm; 13. Internal transmission gear; 14. Mechanism box; 15. Electric or hydraulic mechanism. DETAILED DESCRIPTION

[0034] The present invention will be described in further detail below. Unless otherwise specified, the instruments or materials used in the present invention are commercially available.

[0035] Embodiment 1:

[0036] like Figure 2 As shown, a composite coating for gears used in power equipment is provided, wherein a zinc-nickel alloy layer 2 and a zinc-nickel-phosphorus amorphous alloy layer 3 are plated on the surface of a gear 1 in sequence, wherein the thickness of the zinc-nickel alloy layer 2 is 5 microns, and the thickness of the zinc-nickel-phosphorus amorphous alloy layer 3 is 10 microns. The mass fraction of nickel in the zinc-nickel alloy layer 2 is 7%, and the rest is zinc; the mass fraction of zinc in the zinc-nickel-phosphorus amorphous alloy layer 3 is 5%, the mass fraction of phosphorus is 8%, and the rest is nickel.

[0037] The zinc-nickel alloy layer 2 is an electroplated layer, and the zinc-nickel-phosphorus amorphous alloy layer 3 is a chemically plated layer. The zinc-nickel-phosphorus amorphous alloy layer 3 has a high phosphorus content and exhibits amorphous characteristics.

[0038] like Figure 3 As shown, a method for preparing a gear composite coating comprises first cleaning and activating the surface of a gear 1, electroplating a zinc-nickel alloy layer 2 on the surface, then chemically plating a zinc-nickel-phosphorus amorphous alloy layer 3, and then performing heat treatment and passivation treatment, including the following steps:

[0039] (1) Clean the surface of the transmission gear 1 made of carbon steel to remove dirt, metal chips and other debris attached to the surface; if there is obvious rust or oxide scale on the surface, use sandblasting or wire brush to remove the rust and oxide scale.

[0040] (2) Degreasing the surface of gear 1, using an alkaline degreasing bath containing detergent, bathing at 80°C for 10 minutes, soaking and wiping the parts until there is no obvious oil stain on the surface. The alkaline bath solution is prepared using NaOH 7.5g / L, Na2CO3 35g / L, Na3PO4·12H2O 15g / L, non-ionic surfactant 7.5g / L, and deionized water is added to the total volume of the solution to 1L. In this embodiment, the non-ionic surfactant is dodecylphenol polyoxyethylene ether (OP-10).

[0041] (3) After degreasing, the gear 1 is cleaned with water. First, it is cleaned with 80°C hot water for 2 minutes, and then rinsed or sprayed with room temperature cold water for 2 minutes. The water should be deionized water or distilled water.

[0042] (4) Acid activation: immerse the gear 1 in a hydrochloric acid solution for 1 minute to remove the slight rust on the surface of the gear 1 and activate the metal. Then, rinse it with deionized water or distilled water for later use.

[0043] (5) Prepare zinc-nickel plating solution. The zinc-nickel plating solution includes 8 g / L ZnO, 10 g / L NiSO4·6H2O, 80 g / L NaOH, 20 g / L sodium citrate, 20 g / L triethanolamine, 0.2 g / L vanillin, and the rest is deionized water. When preparing, be careful to prevent precipitation, stir while adding, and heat to 70°C.

[0044] (6) Place the prepared zinc-nickel plating solution in the electroplating tank, with gear 1 as the cathode and the zinc plate as the anode, and immerse in the zinc-nickel plating solution for electroplating. Note that the time from gear 1 being acid-washed to entering the plating tank should not exceed 5 minutes. Control the electroplating current density to 1A / dm 2 , electrochemical deposition time 20min, the coating thickness reaches 5 microns. During the use of the plating solution, water should be added in time, and additives should be added according to the surface quality of the parts and the processing volume. When adding, add less and add more frequently.

[0045] (7) After pre-plating a layer of zinc-nickel alloy coating 2, wash it with 70°C deionized water for 3 minutes. The nickel in the zinc-nickel alloy coating 2 has a certain catalytic activity, and vanillin is also a catalyst. The combination of the two further enhances the catalytic activity of the gear surface, so that it meets the conditions for chemical plating.

[0046] (8) Prepare zinc-nickel-phosphorus plating solution. The zinc-nickel-phosphorus plating solution includes ZnSO4·7H2O 2g / L, NiSO4·7H2O 27g / L, NaH2PO2·H2O 10g / L, sodium citrate 80g / L, NH4Cl 50g / L, 25% NH4OH solution 60mL, and the rest is deionized water. The pH value is controlled at about 8.2 by ammonia water. When preparing, pay attention to prevent precipitation, stir while adding, and heat to 70°C.

[0047] The pH value of the zinc-nickel-phosphorus plating solution ranges from 8.2 to 9.2. Within this range, chemical plating can be carried out smoothly. If it is not within this range, the speed of chemically plating the zinc-nickel-phosphorus amorphous alloy 3 on the gear 1 will be greatly reduced or even difficult to plate.

[0048] (9) Place the prepared zinc-nickel-phosphorus plating solution in a plating tank (there is no zinc-nickel plating solution in the plating tank), and immerse the gear 1 in the zinc-nickel-phosphorus plating solution for chemical plating at a temperature of 90°C for 20 minutes. During the use of the plating solution, add water and additives in time, and add less and more frequently.

[0049] (10) After the chemical plating is completed, clean and dry immediately to remove the plating solution remaining on the surface of the gear 1 to ensure the appearance of the plating layer and prevent unnecessary corrosion.

[0050] (11) Heat treatment after plating, keep constant temperature at 350℃ for 1h. Heat treatment can remove hydrogen atoms in the coating or base metal, eliminate hydrogen embrittlement, and further improve the hardness and corrosion resistance of the composite coating.

[0051] (12) Passivation treatment: use 40g / L H2CrO4, soak the coating at 60℃ for 15min, then wash and dry.

[0052] In this embodiment, a composite coating of an inner zinc-nickel alloy layer 2 and an outer zinc-nickel-phosphorus amorphous alloy 3 is obtained on the surface of the gear 1, with a total thickness of about 15 microns. The mass fraction of nickel in the zinc-nickel alloy layer 2 is about 7%, and the rest is zinc. In the zinc-nickel alloy layer 2, the mass fraction of zinc is about 5%, the mass fraction of phosphorus is about 8%, and the rest is nickel. After testing, the hardness of the gear composite coating of this embodiment is 510HV, and there is still no corrosion after 1500h of neutral salt spray resistance according to GB / T 10125-2012 "Artificial Atmosphere Corrosion Test Salt Spray Test". The two alloy layers of the composite coating of the present invention have good compatibility and complementarity, and the formed composite coating has good hardness, wear resistance and corrosion resistance, which solves the technical problems of insufficient corrosion resistance and hardness of the galvanizing and blackening process on the gear surface in the prior art, and the difficulty of thickening the zinc-nickel-phosphorus amorphous alloy layer 2 on the gear surface and the insufficient corrosion resistance.

[0053] Embodiment 2:

[0054] A composite coating for gears used in power equipment, wherein a zinc-nickel alloy layer 2 and a zinc-nickel-phosphorus amorphous alloy layer 3 are sequentially plated on the surface of a gear 1, wherein the zinc-nickel alloy layer 2 has a thickness of 15 microns, and the zinc-nickel-phosphorus amorphous alloy layer 3 has a thickness of 15 microns. The mass fraction of nickel in the zinc-nickel alloy layer 2 is 11%, and the rest is zinc; the mass fraction of zinc in the zinc-nickel-phosphorus amorphous alloy layer 3 is 8%, the mass fraction of phosphorus is 10%, and the rest is nickel. The zinc-nickel alloy layer 2 is an electroplated layer, and the zinc-nickel-phosphorus amorphous alloy layer 3 is a chemically plated layer.

[0055] A method for preparing a composite coating of a gear for electric power equipment comprises the following steps: firstly cleaning and activating the surface of a gear 1, electroplating a zinc-nickel alloy layer 2 on the surface, then chemically plating a zinc-nickel-phosphorus amorphous alloy layer, and then performing heat treatment and passivation treatment.

[0056] (1) Clean the surface of the transmission gear 1 made of low alloy steel to remove dirt, metal chips and other debris attached to the surface;

[0057] (2) Degreasing the surface of gear 1, using an alkaline degreasing bath containing detergent, bathing at 70°C for 5 minutes, soaking and wiping gear 1 until there is no obvious oil stain on the surface. The alkaline bath solution is prepared using NaOH 15g / L, Na2CO3 45g / L, Na3PO4·12H2O 30g / L, non-ionic surfactant 7.5g / L, and deionized water is added to a total volume of 1L. In this embodiment, the non-ionic surfactant is dodecylphenol polyoxyethylene ether (OP-10).

[0058] (3) After degreasing, the gear 1 is cleaned with water, first with 70°C hot water for 2 min, and then with room temperature cold water for 2 min. The water used is deionized water.

[0059] (4) Acid activation: immerse the gear 1 in a hydrochloric acid solution for 1 min to remove the slight rust on the surface of the gear 1 and activate the metal, then rinse it with deionized water for later use;

[0060] (5) Prepare zinc-nickel plating solution. The zinc-nickel plating solution includes 15 g / L ZnO, 20 g / L NiSO4·6H2O, 150 g / L NaOH, 60 g / L sodium citrate, 60 g / L triethanolamine, 0.1 g / L vanillin, and the rest is deionized water. When preparing, be careful to prevent precipitation, stir while adding, and heat to 60°C.

[0061] (6) Place the prepared zinc-nickel plating solution in the electroplating tank, with gear 1 as the cathode and the zinc plate as the anode, and immerse them in the plating solution for electroplating. Note that the time from gear 1 being acid-washed to entering the plating tank should not exceed 5 minutes. Control the electroplating current density to 5A / dm 2 , electrochemical deposition time 40min, the coating thickness reaches 15 microns. During the use of the plating solution, water should be added in time, and additives should be added according to the surface quality of the parts and the processing volume. When adding, add less and add more frequently.

[0062] (7) After pre-plating the zinc-nickel alloy layer 2, rinse with deionized water for 3 minutes at 80°C and set aside.

[0063] (8) Prepare zinc-nickel-phosphorus plating solution. The zinc-nickel-phosphorus plating solution includes 15 g / L ZnSO4·7H2O, 35 g / L NiSO4·7H2O, 10 g / L NaH2PO2·H2O, 90 g / L sodium citrate, 50 g / L NH4Cl, 60 mL 25% NH4OH solution, and the rest is deionized water. The pH value is controlled at about 9.2 by ammonia water. When preparing, be careful to prevent precipitation, stir while adding, and heat to 70°C.

[0064] (9) Place the prepared zinc-nickel-phosphorus plating solution in a plating tank (there is no zinc-nickel plating solution in the plating tank), and immerse gear 1 in the zinc-nickel-phosphorus plating solution for chemical plating at 98°C for 2 hours. During the use of the zinc-nickel-phosphorus plating solution, water should be added in time, and additives should be added according to the surface quality of the parts and the consumption of the plating solution. When adding, add less and add more frequently.

[0065] (10) After the chemical plating is completed, the gear 1 is immediately cleaned and dried to remove the plating solution remaining on the surface.

[0066] (11) After plating, heat treatment is carried out at a constant temperature of 200°C for 3 hours.

[0067] (12) Passivation treatment: use 20% CrO3 solution to immerse the coating at 85°C for 1 min, then wash and dry.

[0068] In this embodiment, a composite coating of an inner zinc-nickel alloy layer 2 and an outer zinc-nickel-phosphorus amorphous alloy 3 is obtained on the surface of the gear 1, with a total thickness of about 30 microns. The zinc-nickel alloy layer 2 has a nickel mass fraction of 11%, and the rest is zinc. The outer zinc-nickel-phosphorus amorphous alloy 3 has a zinc mass fraction of 8%, a phosphorus mass fraction of 10%, and the rest is nickel.

[0069] After testing, the composite coating of the gear for power equipment prepared in this embodiment has a hardness of 530 HV, and is resistant to neutral salt spray for 1800 hours without corrosion according to GB / T 10125-2012 "Artificial atmosphere corrosion test salt spray test".

[0070] Comparative Example 1:

[0071] The method for preparing a gear coating for electric power equipment in this comparative example is substantially the same as that in Example 1, except that there is no electroplated zinc-nickel alloy layer 2 on the surface, but a direct chemical zinc-nickel-phosphorus amorphous alloy layer 3 is chemically plated, comprising steps (1)-(4) and steps (8)-(12).

[0072] After testing, it is found that no zinc-nickel-phosphorus amorphous alloy layer 3 is formed on the surface of the gear 1 of this comparative example, and the hardness and corrosion resistance are not as good as those of Example 1. This is because the surface activity of the gear 1 is not enough, and a zinc-nickel-phosphorus amorphous alloy layer 3 cannot be directly chemically plated on the surface of the gear 1.

[0073] Comparative Example 2:

[0074] The method for preparing a gear coating for electric equipment in this comparative example is substantially the same as that in Example 1, except that the zinc-nickel plating solution does not contain the catalyst vanillin.

[0075] Upon testing, it was found that a zinc-nickel alloy layer 2 was formed on the surface of the gear 1 in this comparative example, but the thickness of the formed zinc-nickel-phosphorus amorphous alloy layer 3 was less than 5 microns, resulting in the final coating having a lower hardness and corrosion resistance than that of Example 1. This is because although the zinc-nickel alloy layer 2 catalytically activated the surface of the gear 1, the degree of catalytic activation was not sufficient to thicken the zinc-nickel-phosphorus amorphous alloy layer 3. Vanillin can make the nickel of the zinc-nickel alloy layer 2 form a porous structure, thereby increasing the activity of the surface of the gear 1 and facilitating chemical plating of a thicker zinc-nickel-phosphorus amorphous alloy layer 3.

[0076] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the technical content disclosed above without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should fall within the scope of protection of the technical solution of the present invention.

Claims

1. A composite coating for gears used in power equipment, characterized in that: The invention comprises a zinc-nickel alloy layer (2) and a zinc-nickel-phosphorus amorphous alloy layer (3) which are plated on the surface of a gear (1) in sequence, wherein the zinc-nickel alloy layer (2) has a thickness of 5 to 15 microns, and the zinc-nickel-phosphorus amorphous alloy layer (3) has a thickness of 10 to 20 microns. The zinc-nickel alloy layer (2) is an electroplated layer, and the zinc-nickel-phosphorus amorphous alloy layer (3) is a chemically plated layer.

2. The composite coating for gears for electric power equipment according to claim 1, characterized in that: The zinc-nickel alloy layer (2) has a nickel mass fraction of 5% to 15% and the remainder is zinc; the zinc-nickel-phosphorus amorphous alloy layer (3) has a zinc mass fraction of 5% to 15%, a phosphorus mass fraction of 7% to 14% and the remainder is nickel.

3. A method for preparing a composite coating of a gear for electric power equipment, characterized in that: The following steps are involved: A1. Remove impurities from the surface of the gear (1) and perform activation treatment; A2, using the gear (1) as a cathode and immersing it in a zinc-nickel plating solution with an anode for electroplating, forming a zinc-nickel alloy layer (2) on the surface of the gear (1), and cleaning the gear (1); A3, immersing the gear (1) in a zinc-nickel-phosphorus plating solution for chemical plating to form a zinc-nickel-phosphorus amorphous alloy layer (3) on the zinc-nickel alloy layer (2), and cleaning the gear (1); A4. After heat treatment, the gear (1) is immersed in a passivation solution for passivation treatment to obtain a composite coating for gears for electric power equipment.

4. The preparation method according to claim 3, characterized in that: In step A2, the raw materials of the zinc-nickel plating solution include the following components: ZnO 8-15 g / L, NiSO4·6H2O 10-20 g / L, NaOH 80-150 g / L, sodium citrate 20-60 g / L, triethanolamine 20-60 g / L, vanillin 0.1-0.2 g / L, and the rest is deionized water or distilled water.

5. The preparation method according to claim 4, characterized in that: In step A2, during the electroplating process, the current density is 1 to 5 A / dm 2 , time 20 to 40 minutes.

6. The preparation method according to claim 3, characterized in that: In step A3, the raw materials of the zinc-nickel-phosphorus plating solution include the following components: ZnSO4·7H2O 2-15g / L, NiSO4·7H2O 27-35g / L, NaH2PO2·H2O 10g / L, sodium citrate 80-90g / L, NH4Cl 50g / L, 25% NH4OH solution 60mL, and the rest is deionized water or distilled water, and the pH value of the zinc-nickel-phosphorus plating solution is 8.2-9.

2.

7. The preparation method according to claim 6, characterized in that: In step A3, during the chemical plating treatment, the temperature is 90-100° C. and the time is 20 min-2 h.

8. The preparation method according to any one of claims 3 to 7, characterized in that: In step A4, the heat treatment temperature is 200-350° C., and the time is 1-3 hours; the passivation solution is a chromate or chromium-free passivation agent solution, and the passivation treatment time is 1-15 minutes.

9. The preparation method according to any one of claims 3 to 7, characterized in that: In step A1, the impurities include pollutants, oxides and oil.

10. The preparation method according to claim 9, characterized in that: In step A1, removing the impurity oil comprises the following steps: immersing the gear (1) in an alkaline bath at 70 to 80° C. for 1 to 10 minutes; The raw materials of the alkaline bath liquid include the following components: NaOH 7.5-15 g / L, Na2CO3 35-45 g / L, Na3PO4·12H2O 15-30 g / L, non-ionic surfactant 7.5 g / L, and the rest is deionized water or distilled water.

Citation Information

Cited By

  • Mechanism output shaft for power equipment, preparation method and application

    CN119287466A