Efficient metal cluster coupled monatomic catalyst as well as preparation method and application thereof

The Ru/Co1-NCP catalyst prepared by using calcination method in the electrolytic water hydrogen production reaction has solved the problems of insufficient catalytic activity and high cost of precious metal catalysts, and achieved efficient and stable hydrogen generation, which is suitable for seawater electrolysis.

CN119040953APending Publication Date: 2024-11-29ZHENGZHOU UNIV

Patent Information

Application Number
CN202410980789.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing electrolytic water hydrogen production reaction (HER) catalysts are insufficient in catalytic activity under alkaline conditions, especially in seawater applications, and the high cost and poor stability of precious metal catalysts limit their commercial applications.

Method used

The high-efficiency metal cluster coupled single-atom catalyst Ru/Co1-NCP was prepared by calcination method, and a single-atom Co1-NCP carrier was obtained by MOF pyrolysis and loaded with Ru nanoparticles. Doped with phosphorus elements to form graphite-like structures containing Co-N4P ene support, regulates the charge density and structure of the catalyst.

Benefits of technology

It significantly improves the HER reaction activity and stability, reduces the catalyst cost, has excellent electrochemical active area and long cycle life, is better than commercial Pt/C catalysts, and is suitable for alkaline, alkaline seawater and acidic conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040953A_ABST
    Figure CN119040953A_ABST
Patent Text Reader

Abstract

The invention relates to an efficient metal cluster coupled monatomic catalyst as well as a preparation method and application thereof, and belongs to the technical field of catalysts. The molecular formula of the catalyst is Ru / Co1-NCP, and the structure of the catalyst is that ultra-small Ru nanoparticles are loaded on a monatomic Co1-NCP carrier obtained by MOF pyrolysis and P doping. The preparation method comprises the following steps: firstly synthesizing a Co-ZIF-8 material, specifically, dissolving cobalt nitrate hexahydrate, zinc nitrate hexahydrate and dimethylimidazole in a methanol solution, stirring for 24 hours, washing and drying to obtain the Co-ZIF-8 material; pyrolyzing the synthesized Co-ZIF-8 at 950 DEG C under the condition of Ar gas, and pickling with hydrochloric acid to obtain monatomic Co1-NC; then, phosphating in a tubular furnace to obtain a Co1-NCP structure; and finally, reacting with RuCl3 for 12 hours, washing, drying, and reducing for 2 hours under the conditions of Ar / H2 and 300 DEG C to obtain Ru / Co1-NCP. The chemical property of the nanocluster is precisely regulated and controlled by utilizing the pyrolysis method, the overpotential of the prepared catalyst is only 14 mV under the alkaline condition, and the catalyst has excellent HER catalytic activity under alkaline, alkaline seawater, acidic electrolytes and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a high-efficiency metal cluster coupled single atom catalyst and a preparation method and application thereof. Background Art

[0002] As the shortage of fossil energy and environmental pollution become increasingly serious, alternative and pollution-free new energy sources are being studied. Hydrogen has the advantages of high calorific value, no pollution, and good prospects, and has attracted widespread attention, especially the process application research of hydrogen production by electrolysis of seawater. In the process of water electrolysis, the hydrogen evolution reaction (HER) that produces hydrogen occurs at the cathode. However, due to the slow kinetics of HER, its overpotential is high, which affects the hydrogen production rate and wastes power, limiting the commercialization of hydrogen production by electrolysis of water. At present, the HER electrocatalysts used commercially are Pt-based precious metals, and their high cost and poor stability have become limiting factors.

[0003] Among the precious metals, Ru metal is cheaper and has an electronic structure similar to that of Pt, making it a promising alternative to hydrogen evolution catalysts. In addition, reducing the amount of catalyst used and improving atomic utilization is one of the research directions of precious metal catalysts. At present, the morphology of catalysts has shifted from bulk to nano, cluster, single atom, etc. Among them, nanocatalysts have a variety of structures and forms, which are rich and adjustable. Compared with cluster and single atom catalysts, nanocatalysts have higher metal loading, simpler synthesis conditions, and are easy to process, providing a feasible solution for the rapid development of hydrogen evolution catalysts.

[0004] Chinese patent CN114752962A discloses a method for preparing a spider-nest composite carbon nanomaterial @ ruthenium nanoparticles. The preparation process adopts chemical vapor deposition, with MOF-derived spider-nest iron-cobalt alloy nitrogen-doped carbon nanomaterial as the conductive network and ruthenium nanoparticles as the carrier. However, the synthesis technology is relatively complex, the catalytic performance of the catalyst needs to be improved, and it fails to meet the process requirements for electrolysis of seawater.

[0005] Therefore, it is imperative for scientific and technological workers in this field to research and develop alkaline seawater HER catalysts with simple synthesis methods. Summary of the invention

[0006] In view of the defects and shortcomings of the above-mentioned prior art, the present invention provides a highly efficient metal cluster coupled single atom catalyst Ru / Co1-NCP for HER reaction and its preparation method and application, which solves the problems of insufficient catalytic activity of the catalyst under alkaline conditions and limited electrolyte conditions, especially the application to seawater. The preparation method of the present invention mainly adopts calcination, and the synthesis is simple.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A highly efficient metal cluster coupled single atom catalyst, wherein the molecular formula of the catalyst is Ru / Co1-NCP, and the structure is that ultra-small Ru nanoparticles are loaded on a single atom Co1-NCP carrier obtained by MOF pyrolysis and P doping, wherein the Co1-NCP is a graphene-like carrier containing a Co-N4P structure.

[0009] Preferably, the particle size of the Ru nanoparticles is 1 nm-3 nm.

[0010] A method for preparing a highly efficient metal cluster coupled single atom catalyst comprises the following steps:

[0011] S1, dissolve 1.8-13g Zn(NO3)2·6H2O and 0.04-0.4g Co(NO3)2·6H2O in 50mL methanol solution, recorded as solution I;

[0012] S2, dissolving 2.4-15 g of 2-methylimidazole in 50 mL of methanol solution, recorded as solution II;

[0013] S3, slowly add solution II to solution I while stirring, and after the addition is complete, stir the reaction at room temperature for 24 hours to obtain a purple precipitate;

[0014] S4, washing the precipitate prepared in S3 several times by centrifugation with methanol, and drying under vacuum at 60°C for 12 h to obtain Co-ZIF-8;

[0015] S5, placing the Co-ZIF-8 dried in S4 in a tube furnace, heating it at a rate of 5°C / min under argon gas, heating it to 950°C and keeping it for 2h to obtain black powder Co-NC;

[0016] S6, ultrasonically disperse the Co-NC obtained in S5 in 10-30 mL 2M HCl solution, place in a 60°C water bath and stir for 8 h; after acid washing is complete, centrifuge, wash with deionized water and ethanol until neutral, and dry in a vacuum drying oven at 60°C for 12 h to obtain Co1-NC;

[0017] S7, 0.01-0.1g Co1-NC and 0.1-1g NaH2PO2 were placed in a tube furnace, heated at a heating rate of 5°C / min under argon conditions, heated to 300°C and kept warm for 2h; then naturally cooled to room temperature to obtain black powder Co1-NCP;

[0018] S8, measure 100-1000 μL of 10-30 mM RuCl3 solution, ultrasonically disperse it in 40 mL of deionized water, and stir it at room temperature for 30 min; then add 10-50 mg Co1-NCP while stirring, and then stir and react at room temperature for 12 h to obtain a black precipitate;

[0019] S9, centrifuge the black precipitate prepared in S8, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 60°C for 12h;

[0020] S10. Place the dried black solid from S9 in a tube furnace and continuously introduce H2 / Ar (H2 accounts for 10%), heat it at a rate of 5°C / min, heat it to 350°C and keep it for 2h; then cool it naturally to room temperature to obtain black powder Ru / Co1-NCP.

[0021] Preferably, in S7, NaH2PO2 is placed upstream.

[0022] Preferably, the amount of Ru in the Ru / Co1-NCP prepared by the preparation method is 3 wt %.

[0023] The above-mentioned high-efficiency metal cluster-coupled single-atom catalyst is used in industrial alkaline water electrolysis and seawater hydrogen production.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention creatively designs a Ru ultra-small nanoparticle catalyst based on MOF pyrolysis loading, which includes the processes of obtaining a single-atom Co1-NC carrier by pyrolysis of MOF, phosphating the carrier, and loading Ru nanoparticles on the carrier, wherein Co1-NCP is a graphene-like carrier containing a Co-N4P structure. Through the coupling synergy between Co1-NCP and Ru nanoparticles, not only the agglomeration effect of the Ru nanoparticle catalyst itself is overcome, the size of the Ru particles is regulated, but also the charge density around the Ru particles is improved, which is conducive to the adsorption and desorption of hydrogen and enhances the HER reaction activity. The single-atom Co1-NC and the later doped P are obtained by pyrolyzing ZIF-8 containing Co atoms, which regulates the charge density distribution of the carbon component, enhances the adsorption and restriction of Ru nanoparticles, and the porous carbon carrier structure improves the mass transfer of the reaction process.

[0026] 2. The present invention only uses pyrolysis to prepare HER catalysts under three conditions: alkaline, alkaline seawater, and acidic. By precisely controlling the ratio of Co / Zn salts, the content of phosphorus and ruthenium in the precursor solution, the doping levels of cobalt, phosphorus, and ruthenium atoms in the main structure are controlled, thereby guiding the generation of cobalt single atoms, the regulation of phosphorus, and the formation of a large number of ruthenium active sites. The pyrolysis method is simple, easy to control the operation, and easy to be applied in actual production.

[0027] 3. The catalyst of the present invention has low cost, good performance and application performance. The Ru / Co1-NCP catalyst with low metal content has a large electrochemical active area, excellent HER activity and good stability. In 1M KOH electrolyte, the current density is 10mA·cm -2 The overpotential under 1000 ℃ is 14mV, which is better than commercial Pt / C (18mV). At the same time, the activity is also excellent under alkaline seawater and acidic conditions. The Ru / Co1-NCP catalyst is used in the cathode of water electrolysis, with good activity and a cycle life of up to 50h, and also has good stability under high current density. The successful synthesis of this catalyst solves the problem of expensive cost and poor stability of precious metal Pt / C catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Scanning electron microscope images (SEM) of Ru / Co1-NCP (Example 1), Co-ZIF-8 (Comparative Example 1), Co1-NC (Comparative Example 2), and Co1-NCP (Comparative Example 3);

[0029] Figure 2 Transmission electron microscopy (TEM) images of Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), and Co1-NCP (Comparative Example 3);

[0030] Figure 3 X-ray powder diffraction patterns (XRD) of Ru / Co1-NCP (Example 1), Co-ZIF-8 (Comparative Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), and NC (Comparative Example 6);

[0031] Figure 4 X-ray photoelectron spectroscopy (XPS) of Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), and Co1-NCP (Comparative Example 3);

[0032] Figure 5 A comparison chart of alkaline HER performance of Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), Ru / NCP (Comparative Example 4), Ru / Co-NC (Comparative Example 5), NC (Comparative Example 6) and 20% Pt / C;

[0033] Figure 6 A comparison chart of the alkaline seawater HER performance of Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), Ru / NCP (Comparative Example 4), Ru / Co1-NC (Comparative Example 5), NC (Comparative Example 6) and 20% Pt / C;

[0034] Figure 7 A comparison chart of acidic HER performance of Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), Ru / NCP (Comparative Example 4), Ru / Co1-NC (Comparative Example 5), NC (Comparative Example 6) and 20% Pt / C;

[0035] Figure 8 It is a schematic diagram of the preparation method of the present invention. DETAILED DESCRIPTION

[0036] In the present invention, the pH of alkaline seawater is 9-13, and the pH under acidic conditions is 13.

[0037] To make the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0038] Example 1

[0039] A highly efficient metal cluster coupled single atom catalyst, the molecular formula of the catalyst is Ru / Co1-NCP, the structure is that ultra-small Ru nanoparticles (1nm-3nm) are loaded on a single atom Co1-NCP carrier obtained by MOF pyrolysis and P doping, and Co1-NCP is a graphene-like carrier containing a Co-N4P structure.

[0040] Preparation method Figure 8 As shown, it includes the preparation of Co-ZIF-8, pyrolysis of Co-ZIF-8 to obtain a single-atom Co1-NC carrier, phosphating the carrier to obtain Co1-NCP, and loading Ru nanoparticles on the carrier to obtain Ru / Co1-NCP. The specific process is as follows:

[0041] S1, dissolve 3.75g Zn(NO3)2·6H2O and 0.068g Co(NO3)2·6H2O in 50mL methanol solution, recorded as solution I;

[0042] S2, dissolving 4.35 g of 2-methylimidazole in 50 mL of methanol solution, recorded as solution II;

[0043] S3, slowly add solution II to solution I while stirring, and after the addition is complete, stir the reaction at room temperature for 24 hours to obtain a purple precipitate;

[0044] S4, washing the precipitate prepared in S3 several times by centrifugation with methanol, and drying under vacuum at 60°C for 12 h to obtain Co-ZIF-8;

[0045] S5, placing the Co-ZIF-8 dried in S4 in a tube furnace, heating it at a rate of 5°C / min under argon gas, heating it to 950°C and then keeping it at that temperature for 2h to obtain black powder Co-NC;

[0046] S6, ultrasonically dispersing the Co-NC obtained in S5 in 20 mL of 2M HCl solution, placing in a 60°C water bath and stirring for 8 h; after acid washing is complete, centrifugation is performed, washing with deionized water and ethanol until neutral, and drying in a vacuum drying oven at 60°C for 12 h to obtain Co1-NC;

[0047] S7, 0.08g Co1-NC and 0.8g NaH2PO2 were placed in a tube furnace (NaH2PO2 was placed upstream), and the temperature was increased at a rate of 5°C / min under argon gas conditions, and the temperature was increased to 300°C and kept at that temperature for 2h; then the temperature was naturally cooled to room temperature to obtain black powder Co1-NCP;

[0048] S8, measure 690 μL of 20 mM RuCl3 solution, ultrasonically disperse it in 40 mL of deionized water, and stir it at room temperature for 30 min; then add 40 mg Co1-NCP while stirring, and then stir and react at room temperature for 12 h to obtain a black precipitate;

[0049] S9, centrifuge the black precipitate prepared in S8, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 60°C for 12h;

[0050] S10. Place the dried black solid from S9 in a tube furnace and continuously introduce H2 / Ar (H2 accounts for 10%), heat it at a rate of 5°C / min, heat it to 350°C and keep it for 2h; then cool it naturally to room temperature to obtain black powder Ru / Co1-NCP.

[0051] Comparative Example 1

[0052] The difference from Example 1 is that the synthesis is only performed up to step S4. The target product obtained is Co-ZIF-8.

[0053] Comparative Example 2

[0054] The difference from Example 1 is that the synthesis is only performed up to step S6. The target product obtained is Co1-NC.

[0055] Comparative Example 3

[0056] The difference from Example 1 is that the synthesis is only performed up to step S7. The target product obtained is Co1-NCP.

[0057] Comparative Example 4

[0058] The difference from Example 1 is that in step S1, Co(NO3)2·6H2O is not added, and the rest is the same as Example 1. The target product obtained is Ru / NCP.

[0059] Comparative Example 5

[0060] The difference from Example 1 is that the S7 phosphating step is not performed, and the rest is the same as Example 1. The target product obtained is Ru / Co1-NC.

[0061] Comparative Example 6

[0062] The difference from Example 1 is that in step S1, Co(NO3)2·6H2O is not added, and steps S7, S8, S9, and S10 are not performed, and the rest are the same as in Example 1. The target product obtained is NC.

[0063] Catalyst structure characterization

[0064] Figure 1 For the catalyst Ru / Co1-NCP (Example 1- Figure 1 d), Co-ZIF-8 (Comparative Example 1- Figure 1 a), Co1-NC (Comparative Example 2- Figure 1 b), Co1-NCP (Comparative Example 3- Figure 1 c) SEM image of the sample. Figure 1 (a) shows a regular dodecahedron structure of approximately 600 nm in size, indicating the successful synthesis of ZIF-8. Figure 1 (bd) It can be seen that after the cobalt-containing ZIF-8 is pyrolyzed, doped with P and in-situ adsorption and reduction of Ru, the surface structure gradually becomes rough, but no obvious collapse occurs, indicating that the catalyst structure has good stability.

[0065] Figure 2 For the catalyst Ru / Co1-NCP (Example 1- Figure 2 f), Co1-NC (Comparative Example 2- Figure 2 d), Co1-NCP (Comparative Example 3- Figure 2 e) TEM image, where Figure 2 g is Figure 2 (f) Magnified image of the black area. Figure 2 (df) are high-resolution transmission electron microscopy (HRTEM) characterizations of the three samples. Figure 2 In (d, e), Co1-NC and Co1-NCP do not have obvious metal lattice structures, indicating that Co may be a single atom. Figure 2 (f) Nanoparticles with an average particle size of 2 nm were observed. Further analysis of the nanoparticles revealed Figure 2(g) The presence of 0.218 nm lattice fringes corresponding to the (002) crystal plane of Ru indicates the successful preparation of ultrasmall Ru nanoparticles. Figure 2 h shows the uniform distribution of elements in Ru / Co1-NCP catalyst.

[0066] Figure 3 The XRD images of the catalysts Ru / Co1-NCP (Example 1), Co-ZIF-8 (Comparative Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), and NC (Comparative Example 6) are shown in FIG. Figure 3 In the figure, the pattern of Co-ZIF-8 is almost identical to that of standard ZIF-8, indicating the successful synthesis of the ZIF-8 structure. Figure 3 It shows that Ru / Co1-NCP, Co1-NC, Co1-NCP, and NC all have a broad peak (002) of amorphous carbon, and no peaks of cobalt and cobalt oxide, indicating that cobalt may exist in the form of a single atom. In addition, Co-ZIF-8 and Co1-NC have a broad peak of Co2N (111) crystal plane at 42.66°, indicating the existence of Co-N structure and low content. Ru / Co1-NCP has a broad peak of Ru (101) crystal plane at 43.43°, which also confirms the existence of Ru nanoparticles.

[0067] Figure 4 The XPS images of catalysts Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), and Co1-NCP (Comparative Example 3) are shown in FIG. Figure 4 In the XPS spectrum of (a), the peaks of the corresponding elements are present in all three samples, among which the Co element is not obvious due to its low content. Figure 4 In the Ru 3p and 3d spectra (b, c), the appearance of the ruthenium zero-valence peak confirms the presence of Ru nanoparticles in the catalyst, and also the presence of RuO on its surface. x / Ru peaks may be due to partial oxidation in air. Figure 4 In the C1s spectrum of (c), the four main C peaks are consistent with the carbon support structure obtained by pyrolysis of ZIF reported in previous literature. Figure 4 The peak of Co 2p spectrum (d) is close to +2 valence, indicating that Co exists in single atom form and there is no metallic bond. The shift of binding energy position among the three samples indicates that Co may have transferred electrons to Ru. Figure 4 In the N1s spectrum of (e), the peaks of pyridinic nitrogen, metallic nitrogen, pyrrolic nitrogen, graphitic nitrogen, and oxidized nitrogen can be separated. In the three samples, the content of pyridinic nitrogen gradually increases, and this trend is conducive to the occurrence of HER reaction. The appearance of metallic nitrogen proves that metal Co exists mainly in the form of Co-N bonds in the catalyst. Figure 4In the P 2p spectrum of (f), the two peaks of P indicate that P is only bonded to N and not to metal. Therefore, we believe that the doping of P mainly forms the structure of Co-N4P. The above XPS data show the existence of Co single atoms, P doping and the generation of Ru nanoparticles in the catalyst Ru / Co1-NCP.

[0068] Catalyst HER electrochemical performance test

[0069] The prepared catalysts Ru / Co1-NCP (Example 1), Co1-NC (Comparative Example 2), Co1-NCP (Comparative Example 3), Ru / NCP (Comparative Example 4), Ru / Co1-NC (Comparative Example 5), NC (Comparative Example 6) and 20% Pt / C were tested in a CHI 660E electrochemical workstation under the conditions of: temperature 25°C. 3 mg of catalyst, 500 μL of anhydrous ethanol and 50 μL of Nafion solution (5wt%) were slurried and ultrasonicated for more than 60 minutes to form a uniform mixed solution, and 5 μL was drawn and dropped on a platinum carbon electrode for testing. A platinum carbon electrode was used as a working electrode, a carbon rod as a counter electrode, and a calomel electrode (Hg / Hg2Cl2) as a reference electrode to form a three-electrode system, which was tested in 1M KOH, 1M KOH + seawater (seawater comes from the Bohai Sea waters of China) and 0.5M H2SO4 electrolyte.

[0070] Figure 5 The electrochemical test results of alkaline HER of different catalysts are shown in Figure 2. Figure 5 It can be seen from (ad, g, i) that among all the samples, Ru / Co1-NCP (Example 1) has the best catalytic activity at 10 mA cm -2 Under the current condition, the overpotential is only 14mV and the Tafel slope is only 33mV dec-1, which is better than 20% Pt / C (18mV, 35mV dec-1). -1 In addition, Ru / Co1-NCP has the best performance in electrochemical impedance spectroscopy (EIS), electric double layer capacitance (Cdl), and electrochemically active surface area (ECSA) tests, and also has obvious advantages in comparison with similar catalysts reported so far. Figure 5 (h) shows that the catalyst has a Faradaic efficiency close to 100%, indicating that the selectivity of the catalyst is also excellent. Figure 5 (e) shows that the catalytic activity of Ru / Co1-NCP only slightly weakened after 10,000 CV cycles; Figure 5 (f) shows the -2 At a current density of 200 mA·cm -2The good stability of the catalyst under high current density indicates that the catalyst has great potential for practical application.

[0071] Figure 6 , Figure 7 The HER electrochemical test results of different catalysts in alkaline seawater and acidic conditions are shown. Although the performance of Ru / Co1-NCP (Example 1) is not as good as 20% Pt / C, it still has good catalytic activity, especially in alkaline seawater electrolyte. Using abundant seawater for electrolysis to generate hydrogen and combining it with electricity obtained from new energy conversion is extremely attractive for future sustainable development.

[0072] The HER electrochemical test results of Example 1 and Comparative Examples 2-6 are shown in Table 1.

[0073] Table 1 HER electrochemical test results of Example 1 and Comparative Examples 2-6

[0074]

[0075] According to Table 1, the following results can be obtained: ① From Comparative Example 3, it can be seen that if the catalyst component does not contain ruthenium nanoparticles, the performance of the obtained catalyst is very poor; ② From Comparative Example 4, it can be seen that if the catalyst does not contain single-atom cobalt, the catalyst activity will be weakened to a certain extent; ③ From Comparative Example 5, it can be seen that the performance of the catalyst can be regulated by doping with phosphorus; ④ From the comparison of alkaline, alkaline seawater and acidic conditions, it can be seen that the catalytic performance is best under alkaline conditions, the catalytic performance of alkaline seawater is slightly weakened, and the catalytic performance is acceptable under acidic conditions.

[0076] With the above-mentioned ideal embodiments of the present invention as inspiration, through the above-mentioned description, relevant staff can make various changes and modifications without departing from the technical idea of ​​the present invention. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims. Any equivalent changes or modifications made according to the spirit of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A highly efficient metal cluster coupled single atom catalyst, characterized in that: The molecular formula of the catalyst is Ru / Co1-NCP, and the structure is that ultra-small Ru nanoparticles are loaded on a single-atom Co1-NCP carrier obtained by pyrolysis of MOF and P doping. Co1-NCP is a graphene-like carrier containing a Co-N4P structure.

2. The efficient metal cluster coupled single atom catalyst according to claim 1, characterized in that: The particle size of the Ru nanoparticles is 1 nm-3 nm.

3. A method for preparing a highly efficient metal cluster coupled single atom catalyst, characterized in that: The preparation method comprises the following steps: S1, dissolve 1.8-13 g Zn(NO3)2·6H2O and 0.04-0.4 g Co(NO3)2·6H2O in 50 mL methanol solution, recorded as solution I; S2, dissolve 2.4-15 g 2-methylimidazole in 50 mL methanol solution, recorded as solution II; S3, slowly add solution II to solution I while stirring, and after the addition is complete, stir the reaction at room temperature for 24 hours to obtain a purple precipitate; S4, washing the precipitate prepared in S3 several times by centrifugation with methanol, and drying under vacuum at 60 °C for 12 h to obtain Co-ZIF-8; S5, placing the Co-ZIF-8 dried in S4 in a tube furnace, heating it at a rate of 5°C / min under argon gas, heating it to 950°C and then keeping it at that temperature for 2 h to obtain black powder Co-NC; S6, ultrasonically disperse the Co-NC obtained in S5 in 10-30 mL 2 M HCl solution, place in a 60°C water bath and stir for 8 h; after acid washing is complete, centrifuge, wash with deionized water and ethanol until neutral, and dry in a vacuum drying oven at 60°C for 12 h to obtain Co1-NC; S7, 0.01-0.1 g Co1-NC and 0.1-1 g NaH2PO2 were placed in a tube furnace, heated at a rate of 5°C / min under argon gas, heated to 300°C and kept at that temperature for 2 h; then cooled to room temperature naturally to obtain black powder Co1-NCP; S8, measure 100-1000 μL of 10-30 mM RuCl3 solution, ultrasonically disperse it in 40 mL of deionized water, and stir it at room temperature for 30 min; then add 10-50 mg Co1-NCP while stirring, and then stir and react at room temperature for 12 h to obtain a black precipitate; S9, centrifuge the black precipitate prepared in S8, wash it with deionized water and ethanol several times, and dry it in a vacuum drying oven at 60°C for 12 h; S10. Place the dried black solid from S9 in a tube furnace and continuously introduce H2 / Ar. Heat the mixture at a rate of 5°C / min. Heat the mixture to 350°C and keep the temperature for 2 h. Then cool the mixture naturally to room temperature to obtain black powder Ru / Co1-NCP.

4. The method for preparing a highly efficient metal cluster coupled single atom catalyst according to claim 3, characterized in that: In S7, NaH2PO2 is placed upstream.

5. The method for preparing a highly efficient metal cluster coupled single atom catalyst according to claim 3, characterized in that: The amount of Ru in the Ru / Co1-NCP prepared by the preparation method is 3 wt %.

6. The method for preparing a highly efficient metal cluster coupled single atom catalyst according to claim 3, characterized in that: The high-efficiency metal cluster coupled single-atom catalyst prepared by the preparation method is applied to industrial alkaline water electrolysis and seawater hydrogen production.

Citation Information

Patent Citations

  • Preparation and application of spider-nest-shaped composite carbon nanomaterial and ruthenium nanoparticles

    CN114752962A

Cited By

  • Porous carbon supported metal monatomic-metal sub-nano cluster synergistic catalyst as well as preparation method and application thereof

    CN122382605A