Additive for electroplating copper, preparation method of additive and electroplating solution

By using a combination additive of surfactant, imidazole ionic liquid, leveling agent and brightener in acid copper plating solution, the component ratio and synergistic effect are optimized, and the problems of surface unevenness and low brightness of acid copper plating solution are solved. , realizes efficient brightness and ductility of electroplating copper coating.

CN119040975APending Publication Date: 2024-11-29SHANGHAI BOSTONE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410682242.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

It is difficult for existing acidic copper plating solution to form a uniform surface, which affects the flatness and brightness of the plating layer and affects the quality of the printed circuit board.

Method used

Using electroplating copper additives containing surfactants, imidazole ionic liquids, leveling agents and brighteners, the brightness and ductility of the electroplating layer are improved by optimizing the mass ratio and synergistic effects of each component, and through specific imidazoles The synergistic effect of ion-like liquids and polyethyleneimine organic amine cationic surfactants enhances the deposition uniformity and current efficiency of copper ions.

Benefits of technology

It significantly improves the brightness and ductility of the electroplating solution, enhances the flatness and current efficiency of the plating layer, and solves the brightness and uniformity of the plating layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of electroplating solutions, in particular to an additive for copper electroplating, a preparation method of the additive and an electroplating solution. The additive for copper electroplating comprises the following components: a surface active agent, imidazolium ionic liquid, a leveling agent and a brightening agent, the imidazolium ionic liquid is selected from a group consisting of 1 to C4-C20 alkyl-3-methylimidazole bromine salts; the surface active agent comprises a cationic surface active agent and a nonionic surface active agent. All the components in the additive have a synergistic effect, so that the additive for electro-coppering has excellent current efficiency, brightness and ductility during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating solutions, and in particular to an additive for copper electroplating, a preparation method thereof, and an electroplating solution. Background Art

[0002] With the development of the electronics industry, the requirements for electronic equipment are getting higher and higher. As one of the components of electronic equipment, the quality of the design of the printed circuit board is related to the quality of the electronic equipment. When preparing the printed plate, the board surface needs to be electroplated first. The most common method is to electroplating copper to form a copper coating. The quality of the copper coating is one of the factors that affect the quality of the printed circuit board.

[0003] The acid copper electroplating solution that is currently used more frequently is not easy to form a uniform surface during the electroplating process, which affects the flatness of the coating. The flatness will affect the brightness of the coating, and the brightness is a technical indicator that must be measured for the coating.

[0004] Therefore, there is an urgent need to develop a new acid copper electroplating solution that has high brightness when used. Summary of the invention

[0005] The first aspect of the present invention provides an additive for copper electroplating, the components of the additive for copper electroplating include: a surfactant, an imidazole ionic liquid, a leveler and a brightener; the imidazole ionic liquid is selected from 1-C4~C20 alkyl-3-methylimidazolium bromide; the surfactant includes a cationic surfactant and a nonionic surfactant.

[0006] The additive for copper electroplating in the present invention can be used in the electroplating solution. The surfactant and the imidazole ionic liquid act together in the electroplating solution system to better improve the performance of the electroplating layer, especially its brightness and ductility.

[0007] In the present invention, in order to better increase the performance of the additive for copper electroplating, preferably, the mass ratio of the ionic liquid to the surfactant is 1:(13-23), for example, 1:13, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23.

[0008] In the present invention, in order to better improve the performance of the additive for copper electroplating, preferably, the mass ratio of the leveling agent to the surfactant is 1:(20-45), for example, 1:20, 1:23, 1:25, 1:30, 1:32, 1:35, 1:38, 1:40, 1:42, 1:45.

[0009] In the present invention, in order to better improve the performance of the additive for copper electroplating, preferably, the mass ratio of the brightener to the surfactant is 1:(130-450), for example, 1:130, 1:133, 1:150, 1:160, 1:200, 1:230, 1:350, 1:400, 1:450.

[0010] In the present invention, the surfactant can increase the wetting ability of the electrolyte on the electrode surface. In order to better increase the synergistic effect of the cationic surfactant and the non-ionic surfactant, as a preferred technical solution of the present invention, the mass ratio of the cationic surfactant to the non-ionic surfactant is 1:(0.1-0.6), for example, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6.

[0011] The cationic surfactant and the nonionic surfactant used in the invention work synergistically with each other in the additive system of the invention, and can better improve the performance of the copper electroplating solution when the additive is used in the copper electroplating solution.

[0012] As a preferred technical solution of the present invention, the cationic surfactant is selected from polyethyleneimine organic amine cationic surfactant.

[0013] The polyethyleneimine organic amine cationic surfactant in the present invention can be obtained from the market, and its preferred model is BASF Lupasol SK.

[0014] As a preferred technical solution of the present invention, the nonionic surfactant is selected from polyethylene glycol and EO-PO block polyether.

[0015] As a preferred technical solution of the present invention, the mass ratio of the polyethylene glycol to the EO-PO block polyether is 1:(0.5-1), for example, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.

[0016] As a preferred technical solution of the present invention, the average molecular weight of the polyethylene glycol is 2000-4000, for example, 2000, 3000, or 4000.

[0017] As a preferred technical solution of the present invention, the number average molecular weight of the EO-PO block polyether is 1000-5000, for example, 1000, 2000, 3000, 4000 or 5000.

[0018] In the present invention, the specific polyethyleneimine organic amine cationic surfactant is used to synergize with polyethylene glycol to better increase the performance of the additive, especially the brightness of the coating when it is used. This may be because the cationic amine, -OH and -O- in the polyethyleneimine organic amine cationic surfactant are electrostatically paired with some intermediates in the common system during copper deposition, making it difficult for copper ions to deposit in high current density areas, which has a leveling effect, and the flatness of the coating is the main reason affecting the brightness of the coating.

[0019] The inventors have found that although the specific surfactant in the present invention can better increase the all-plating ability of the electroplating solution when used in the electroplating solution, it may affect the viscosity of the electroplating solution to a certain extent, thereby reducing the current efficiency. In the present invention, it has been found through research that the use of imidazole ionic liquids can better improve the current efficiency of the electroplating solution during electroplating. The ionic liquid is miscible with water, which can better increase the dispersibility of each component in the system. At the same time, imidazole can weaken the electrostatic coupling strength between the surfactant and the copper surface leveler, further increasing the deposition rate of copper ions.

[0020] As a more preferred technical solution of the present invention, the imidazole ionic liquid is selected from 1-C14~C16 alkyl-3-methylimidazolium bromide.

[0021] In the present invention, the alkyl group in the 1-C4~C20 alkyl-3-methylimidazolium bromide may be a straight-chain alkyl group or a branched-chain alkyl group, and is preferably a straight-chain alkyl group.

[0022] In the present invention, the use of 1-C14~C16 alkyl-3-methylimidazolium bromide can further increase the all-plating ability of the additive when used in the electroplating solution. It is speculated that this is because the long straight-chain alkyl in the ionic liquid can better improve the uniformity of the copper deposition layer, thereby better increasing the flatness of the coating.

[0023] As a preferred technical solution of the present invention, the leveling agent is selected from at least one of 5-amino-1,3,4-thiadiazole-2-sulfonamide, N-(1,3,4-thiadiazole) nicotinamide, sodium mercaptoimidazole propanesulfonate and tetrahydrothiazolidinethione.

[0024] As a more preferred technical solution of the present invention, the leveling agent is selected from 5-amino-1,3,4-thiadiazole-2-sulfonamide.

[0025] In the present invention, the use of 5-amino-1,3,4-thiadiazole-2-sulfonamide as a leveling agent can better cooperate with the surfactant to increase the brightness of the coating.

[0026] As a preferred technical solution of the present invention, the brightener is selected from at least one of 1,4-butynediol, thiourea, sodium 3-mercapto-1-propane sulfonate and sodium dimethylformamidopropane sulfonate, preferably sodium 3-mercapto-1-propane sulfonate and / or sodium dimethylformamidopropane sulfonate.

[0027] The second aspect of the present invention provides a method for preparing the above-mentioned additive for electroplating copper, and the preparation method comprises: mixing a surfactant, an imidazole ionic liquid, a leveling agent and a brightener.

[0028] In the present invention, there is no particular limitation on the mixing method, as long as the mixture can be mixed uniformly, and those skilled in the art can mix the mixture according to conventional methods in the art.

[0029] The third aspect of the present invention provides an electroplating solution, which comprises: the electroplating copper additive described in the first aspect of the present invention, an inorganic acid, chloride ions, a copper salt, and water.

[0030] In the present invention, the additive for copper electroplating of the present invention is used in the electroplating solution, so that the electroplating solution can better increase the performance of the electroplating layer, especially its brightness and ductility, when used.

[0031] As a preferred technical solution of the present invention, the electroplating solution comprises: 430-510 mg / L of the electroplating copper additive described in the first aspect of the present invention, 200-300 g / L of inorganic acid, 50-70 mg / L of chloride ions, 70-80 g / L of copper salt, and the balance is water.

[0032] As a preferred technical solution of the present invention, the inorganic acid is selected from at least one of sulfuric acid, phosphoric acid, nitric acid, aminosulfonic acid, boric acid and fluoroboric acid.

[0033] As a more preferred technical solution of the present invention, the inorganic acid is sulfuric acid.

[0034] The chloride ions in the present invention play an activation role, and those skilled in the art know that the chloride ions are generally provided by hydrochloric acid.

[0035] The copper salt is a component that provides copper ions. The copper salt can be a conventional raw material in the art, and is preferably copper sulfate pentahydrate.

[0036] In the present invention, the electroplating solution can be obtained by mixing the copper electroplating additive described in the first aspect of the present invention, an inorganic acid, chloride ions, a copper salt and water.

[0037] In the present invention, there is no particular limitation on the mixing method, as long as the mixture can be mixed uniformly, and those skilled in the art can mix the mixture according to conventional methods in the art.

[0038] In the present invention, the process of electroplating using the electroplating solution of the present invention comprises: electroplating the workpiece to be electroplated by using a direct current electroplating process in the presence of the electroplating solution of the present invention.

[0039] As a preferred technical solution of the present invention, the electroplating conditions include: first, at 1.5-2 A / dm 2 Electroplating at 20-30 min, then at 3.5-4 A / dm 2 Electroplating for 10-15 min.

[0040] In the present invention, the inventors found that electroplating at a low current density stage and then electroplating at a high current density can not only better increase the current efficiency, but also further increase the ductility of the coating. It is speculated that this is because the growth of high-position copper grains is suppressed in the early stage, and the coating thickness can be better increased in the later stage.

[0041] As a preferred technical solution of the present invention, the electroplating temperature is 10-60°C, preferably 25-45°C.

[0042] In the present invention, specifically, the workpiece to be electroplated is placed in the middle of the copper electroplating additive, connected to the cathode circuit, copper anodes are placed at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, and then the temperature is 10-60°C, preferably 25-45°C, at 1.5-2A / dm 2 Electroplating at 20-30min, then at 3.5-4A / dm 2 Electroplating for 10-15 minutes.

[0043] As a preferred technical solution of the present invention, the electroplating temperature is 10-60°C, preferably 25-45°C.

[0044] Through the above technical solution, the present invention has at least the following technical effects: The components of the present invention cooperate with each other so that when the additive for copper electroplating is used in the electroplating solution, the electroplating solution has excellent current efficiency, brightness and ductility when used. DETAILED DESCRIPTION

[0045] The present invention is described in detail below through examples. The following examples are only illustrative of the specific technical solutions of the present invention and do not limit the scope of the present invention. That is, it should be understood that non-essential simple corrections, adjustments and combinations made by those skilled in the art based on the inventive concept of the present invention are all within the scope of protection claimed by the present invention.

[0046] In the following test example: 1. The test method for brightness is visual inspection. Experienced inspectors in the laboratory use visual inspection to score the appearance of the copper-plated layer of the electroplated samples. The scoring standard is: Level 9, the surface of the coating is as bright as a mirror; Level 8, the surface of the coating is bright; Level 7, the coating has a slight brightness; Level 6, the coating has no metallic luster and has slight pinholes; Level 5, the coating is gray and has pitting.

[0047] 2. Current efficiency = (M2-M1) / M3*100%, where M1 is the mass of the stainless steel plate sample before electroplating, M2 is the mass of the sample after electroplating, and M3 is the theoretical mass that should be deposited with the same amount of electricity.

[0048] 3. Elongation determination: Peel off the coating and test the electroplated copper foil with a ductility tester. D = △L / L × 100%, where D represents the elongation of the coating (%); △L represents the length difference before and after the test of the sample (mm); L is the original length of the sample (mm).

[0049] Example 1 Prepare the following components: sulfuric acid 200 g / L, chloride ion 50 mg / L, copper sulfate pentahydrate 70 g / L, polyethylene glycol (average molecular weight 2000) 50 mg / L, EO-PO block polyether (number average molecular weight 2000) 50 mg / L, polyethyleneimine organic amine cationic surfactant (model BASF Lupasol SK) 300 mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 10 mg / L, sodium 3-mercapto-1-propane sulfonate 1 mg / L, linear hexadecyl-3-methylimidazolium bromide 25 mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 2

[0050] Prepare the following components: sulfuric acid 240g / L, chloride ion 60mg / L, copper sulfate pentahydrate 74g / L, polyethylene glycol (average molecular weight 2000) 100mg / , EO-PO block polyether (number average molecular weight 4000) 60mg / L, polyethyleneimine organic amine cationic surfactant (model BASF Lupasol SK) 280mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 20mg / L, sodium 3-mercapto-1-propane sulfonate 2mg / L, linear hexadecyl-3-methylimidazolium bromide 20mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 3

[0051] Prepare the following components: sulfuric acid 300 g / L, chloride ion 70 mg / L, copper sulfate pentahydrate 80 g / L, polyethylene glycol (average molecular weight 3000) 90 mg / L, EO-PO block polyether (number average molecular weight 2000) 80 mg / L, polyethyleneimine organic amine cationic surfactant (model BASF Lupasol SK) 280 mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 18 mg / L, sodium dimethylformamidopropane sulfonate 3 mg / L, linear tetradecyl 3-methylimidazolium bromide 30 mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 4

[0052] Prepare the following components: 240 g / L sulfuric acid, 60 mg / L chloride ion, 74 g / L copper sulfate pentahydrate, 270 mg / L polyethylene glycol (average molecular weight 2000), 170 mg / L EO-PO block polyether (number average molecular weight 4000), 20 mg / L 5-amino-1,3,4-thiadiazole-2-sulfonamide, 2 mg / L sodium 3-mercapto-1-propane sulfonate, 20 mg / L linear hexadecyl-3-methylimidazolium bromide, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 5

[0053] Prepare the following components: sulfuric acid 240 g / L, chloride ion 60 mg / L, copper sulfate pentahydrate 74 g / L, EO-PO block polyether (number average molecular weight 4000) 160 mg / L, polyethyleneimine organic amine cationic surfactant (model BASF Lupasol SK) 280 mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 20 mg / L, sodium 3-mercapto-1-propane sulfonate 2 mg / L, linear hexadecyl-3-methylimidazolium bromide 20 mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 6

[0054] Prepare the following components: 240 g / L sulfuric acid, 60 mg / L chloride ion, 74 g / L copper sulfate pentahydrate, 160 mg / L polyethylene glycol (average molecular weight 2000), 280 mg / L polyethyleneimine organic amine cationic surfactant (model BASF Lupasol SK), 20 mg / L 5-amino-1,3,4-thiadiazole-2-sulfonamide, 2 mg / L sodium 3-mercapto-1-propane sulfonate, 20 mg / L linear hexadecyl 3-methylimidazolium bromide, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 7

[0055] Prepare the following components: sulfuric acid 240 g / L, chloride ion 60 mg / L, copper sulfate pentahydrate 74 g / L, polyethylene glycol (average molecular weight 2000) 110 mg / L, EO-PO block polyether (number average molecular weight 4000) 70 mg / L, polyethylene imine organic amine cationic surfactant (model BASF Lupasol SK) 280 mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 20 mg / L, 3-mercapto-1-propane sulfonate sodium 2 mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating. Example 8

[0056] Prepare the following components: sulfuric acid 240 g / L, chloride ion 60 mg / L, copper sulfate pentahydrate 74 g / L, polyethylene glycol (average molecular weight 2000) 100 mg / L, EO-PO block polyether (number average molecular weight 4000) 60 mg / L, polyethylene imine organic amine cationic surfactant (model BASF Lupasol SK) 280 mg / L, 5-amino-1,3,4-thiadiazole-2-sulfonamide 20 mg / L, sodium 3-mercapto-1-propane sulfonate 2 mg / L, 1-hexyl-3-methylimidazolium bromide 20 mg / L, and the balance is water; The above components are mixed evenly to obtain an additive for copper electroplating.

[0057] Electroplating Sample Preparation Example 1 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 1 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 30°C, at 1.5A / dm 2 Electroplating for 30 min at 4 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0058] The test showed that the brightness was level 8, the elongation was 31.4%, and the current efficiency was 96%.

[0059] Electroplating Sample Preparation Example 2 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 2 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0060] The test showed that the brightness was level 9, the elongation was 31.2%, and the current efficiency was 95%.

[0061] Electroplating sample preparation example 3 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 3 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 30°C, at 1.6A / dm 2 Electroplating for 30 min at 3A / dm 2 The electroplating was performed for 12 min to obtain an electroplated sample.

[0062] The test showed that the brightness was level 9, the elongation was 30.8%, and the current efficiency was 94%.

[0063] Electroplating Sample Preparation Example 4 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 4 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0064] The test showed that the brightness was level 5, the elongation was 27.4%, and the current efficiency was 89%.

[0065] Electroplating Sample Preparation Example 5 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 5 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0066] The test showed that the brightness was level 6, the elongation was 28.7%, and the current efficiency was 92%.

[0067] Electroplating Sample Preparation Example 6 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 6 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0068] The test showed that the brightness was level 7, the elongation was 29.3%, and the current efficiency was 93%.

[0069] Electroplating Sample Preparation Example 7 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 7 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0070] The test showed that the brightness was level 5, the elongation was 28.8%, and the current efficiency was 74.1%.

[0071] Electroplating Sample Preparation Example 8 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 8 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 Electroplating for 30 min at 3.5 A / dm 2 The electroplating was performed for 10 min to obtain an electroplated sample.

[0072] The test showed that the brightness was level 6, the elongation was 30.9%, and the current efficiency was 94%.

[0073] Electroplating Sample Preparation Example 9 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 2 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 1.5A / dm 2 The electroplating was performed for 40 min to obtain an electroplated sample.

[0074] The test showed that the brightness was level 8, the elongation was 24.3%, and the current efficiency was 84.5%.

[0075] Electroplating Sample Preparation Example 10 Prepare a 40cm*50cm polished stainless steel plate, place the copper electroplating additive in Example 2 in the plating tank, and place the stainless steel plate in the middle of the copper electroplating additive, connected to the cathode circuit, place copper anodes at both ends of the copper electroplating additive, equidistantly opposite to the two sides of the workpiece to be electroplated, and connected to the anode circuit, then at a temperature of 45°C, at 3.5A / dm 2 The electroplating was performed for 40 min to obtain an electroplated sample.

[0076] The test showed that the brightness was level 7, the elongation was 27.4%, and the current efficiency was 87%.

[0077] From the results of the above examples and electroplating sample preparation examples, it can be seen that the electroplating copper additive of the present invention has excellent current efficiency, brightness and ductility when used.

Claims

1. An additive for copper electroplating, characterized in that The components of the additive for electroplating copper include: surfactant, imidazole ionic liquid, leveler and brightener; the imidazole ionic liquid is selected from 1-C4~C20 alkyl-3-methylimidazolium bromide; the surfactant includes cationic surfactant and nonionic surfactant.

2. The additive according to claim 1, characterized in that The mass ratio of the ionic liquid to the surfactant is 1:(13-23); the mass ratio of the leveling agent to the surfactant is 1:(20-45); and the mass ratio of the brightener to the surfactant is 1:(130-450).

3. The additive according to claim 1 or 2, characterized in that The mass ratio of the cationic surfactant to the nonionic surfactant is 1:(0.1-0.6).

4. The additive according to claim 1 or 2, characterized in that The cationic surfactant is selected from polyethyleneimine organic amine cationic surfactants.

5. The additive according to claim 1 or 2, characterized in that The nonionic surfactant is selected from polyethylene glycol and EO-PO block polyether.

6. The additive according to claim 1 or 2, characterized in that The imidazole ionic liquid is selected from 1-C14~C16 alkyl-3-methylimidazolium bromide.

7. The additive according to claim 1 or 2, characterized in that The leveler is selected from at least one of 5-amino-1,3,4-thiadiazole-2-sulfonamide, N-(1,3,4-thiadiazole) nicotinamide, sodium mercaptoimidazole propanesulfonate and tetrahydrothiazolidinethione.

8. The additive according to claim 1 or 2, characterized in that The brightener is selected from at least one of 1,4-butynediol, thiourea, sodium 3-mercapto-1-propane sulfonate and sodium dimethylformamidopropane sulfonate.

9. A method for preparing the additive for copper electroplating according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: mixing a surfactant, an imidazole ionic liquid, a leveling agent and a brightening agent to obtain the product.

10. An electroplating solution, characterized in that: The electroplating solution comprises the electroplating copper additive according to any one of claims 1 to 8, an inorganic acid, chloride ions, a copper salt, and water; The process of electroplating with the electroplating solution comprises: electroplating the workpiece to be electroplated by using a direct current electroplating process in the presence of the electroplating solution.

Citation Information

Cited By

  • Ultrahigh-purity copper sulfate electroplating solution as well as preparation method and application thereof

    CN120738714A

  • High-performance sand acid copper additive and preparation process thereof

    CN120925036A

  • High-performance copper sa acid additive and preparation process thereof

    CN120925036B