Integrated circuit pin welding and tin plating process
Through cleaning, pretreatment, electroplating and heat treatment, combined with crystallization refiners in the electroplating solution, a high-quality pure tin plating layer is formed, solving the problems of lead pollution and poor stability in traditional tin lead plating, achieving higher connection stability and welding performance.
Patent Information
- Application Number
- CN202411180202.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
AI Technical Summary
Lead in traditional tin lead coating is a toxic heavy metal that pollutes the environment and endangers human health and ecosystems. It may cause lead poisoning to welding workers, and it is easy to cause tin migration and whiskers in extreme environments, resulting in short circuits between device pins. Failure, poor stability.
Using an integrated circuit pin welding tin plating process, including cleaning treatment, pre-plating pre-plating, electroplating operation, cleaning, drying and heat treatment, by adding crystallization refining agent to the plating solution and performing three cycles of heat treatment, Form a uniform pure tin coating to improve connectivity and stability.
It effectively avoids tin migration and whisker generation, improves the connection stability of the integrated circuit and the corrosion resistance and wear resistance of the plating layer, ensures soldering quality and reliability, replaces traditional tin-lead plating, and avoids the harm of lead.
Smart Images

Figure CN119040981A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of integrated circuit pin processing, in particular to a tinning process for integrated circuit pin welding. Background Art
[0002] An integrated circuit is a circuit with specific functions that integrates a certain number of commonly used electronic components, such as resistors, capacitors, transistors, etc., as well as the connections between these components, through semiconductor technology. The pins, also known as leads, are the connections between the internal circuit of the integrated circuit and the peripheral circuit. All the pins constitute the interface of the chip. The end of the lead is soldered to form a solder joint with the pad on the printed circuit board. In the post-packaging process of the integrated circuit, a metal coating with good welding performance is usually coated on the surface of the integrated circuit pin. The coating can improve the welding performance of the integrated circuit pin, including increasing the welding contact area, improving welding connectivity, and reducing the welding temperature, thereby ensuring welding quality and reliability.
[0003] At present, the surface of integrated circuit pins is usually coated with tin-lead plating. However, in the processing of traditional tin-lead plating, lead is a toxic heavy metal that will pollute the environment and cause harm to human health and the ecosystem. It is easy to cause lead poisoning for workers engaged in welding operations. In extreme environments of high temperature, high humidity and high pressure, it is easy to cause tin migration and whisker generation, which will cause short circuit failure between device pins and poor stability. Summary of the invention
[0004] The purpose of the present invention is to provide a tin-plating process for integrated circuit pin welding to solve the problem that lead is a toxic heavy metal in the processing of traditional tin-lead plating, which will pollute the environment, cause harm to human health and the ecosystem, and easily cause lead poisoning to workers engaged in welding operations. In extreme environments of high temperature, high humidity and high pressure, tin migration and whisker generation are easily caused, thereby causing short circuit failure between device pins and poor stability.
[0005] To achieve the above object, the present invention provides the following technical solution: a tinning process for integrated circuit pin welding, comprising the following steps:
[0006] S1. Clamp the integrated circuit pins and load them, clean the integrated circuit pins, and remove impurities and oil stains on the surface;
[0007] S2, pre-treatment of the cleaned integrated circuit pins before electroplating, including electrolytic deburring, deoxidation and activation treatment;
[0008] S3, immersing the cleaned and pretreated integrated circuit pins in an electroplating tank containing a crystal refiner, and then performing an electrotin plating operation on the integrated circuit pins, and applying an electric current to deposit tin salt on the surface of the pins to form a uniform tin layer;
[0009] S4, after the electroplating is completed, the integrated circuit pins are taken out for cleaning and washing to remove impurities and solvents remaining in the electroplating solution;
[0010] S5. Dry the processed integrated circuit pins to ensure that the surface is clean and free of water marks;
[0011] S6, heat-treating the integrated circuit pins with tin to ensure that the tin crystals are rearranged without melting the tin, and performing three consecutive cycles of heat treatment;
[0012] S7. After the heat treatment is completed, the integrated circuit pins are tested and packaged after passing the test.
[0013] Preferably, in step S1, the cleaning process of the integrated circuit pins includes the following steps:
[0014] S11. Use chlorine-free detergent and deionized water to put into ultrasonic cleaning machine and set corresponding parameters;
[0015] S12, placing the integrated circuit pins into an ultrasonic cleaning machine, starting the equipment for cleaning, and removing dirt attached to the surface of the integrated circuit pins;
[0016] S13. After cleaning, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the detergent residue is completely removed;
[0017] S14, placing the cleaned integrated circuit pins into a drying device for drying.
[0018] Preferably, in step S2, the pre-plating pretreatment of the cleaned integrated circuit pins comprises the following steps:
[0019] S21, placing the cleaned integrated circuit pins into an electrolytic bath, keeping the pins from contacting each other;
[0020] S22, filling electrolyte to start the electrolytic deburring equipment, applying current and voltage to perform deburring processing;
[0021] S23, placing the deburred integrated circuit pins into a deoxidation device for deoxidation treatment;
[0022] S24, placing the deoxidized integrated circuit pins into an activation tank for activation treatment;
[0023] S25. After the pretreatment is completed, the integrated circuit pins are taken out and rinsed thoroughly with clean water to ensure that the treatment liquid is completely removed.
[0024] Preferably, in step S3, the integrated circuit pin electrotinning operation includes the following steps:
[0025] S31, prepare the electroplating tinning equipment, install the integrated circuit pins to be electroplated in the electroplating fixture or tank, and ensure that the pins do not contact each other;
[0026] S32, adjusting the temperature and concentration of the electroplating solution in the electroplating tank, adding a crystallization refiner into the electroplating solution, and fully mixing the crystallization refiner with the electroplating solution;
[0027] S33, placing the installed pin fixture into the electroplating tank, allowing the pin to be completely immersed in the electroplating solution;
[0028] S34, setting the current density and electroplating time, starting the electroplating equipment, and starting the electroplating process.
[0029] Preferably, in step S34, the current density is 10-20A / dm 2 , the electroplating time is 40-80s.
[0030] Preferably, in step S4, the step of removing the integrated circuit pins for cleaning and washing comprises the following steps:
[0031] S41, placing the electroplated integrated circuit pins into a cleaning tank or cleaning equipment;
[0032] S42, using a cleaning agent to soak and clean the pins for a period of time to remove dirt and impurities remaining in the electroplating solution;
[0033] S43, after cleaning, using a neutralizing agent for neutralization treatment;
[0034] S44. Finally, the cleaned integrated circuit pins are washed with clean water to remove the residue of the cleaning agent.
[0035] Preferably, in step S5, the drying process adopts a hot air drying process, and the specific process includes the following steps:
[0036] S51, placing the tinned integrated circuit pins into a drying oven for drying;
[0037] S52, adjust the drying box temperature to 50-80 degrees Celsius, the drying time to 15-50 minutes, and the wind speed to 1-2 m / s;
[0038] S53. After the drying process is completed, the integrated circuit pins are naturally cooled to room temperature.
[0039] Preferably, in step S6, the heat treatment comprises the following steps:
[0040] S61, placing the tin-plated integrated circuit pins into a heat treatment furnace for preheating;
[0041] S62, setting the heat treatment temperature and time of the heat treatment furnace to perform heat treatment;
[0042] S63, after the heat treatment is completed, the integrated circuit pins are naturally cooled;
[0043] S64, repeat steps S61-S63 three times to complete the heat treatment.
[0044] Preferably, in step S61, the preheating temperature is 160-218°C.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] 1. In the present invention, three cycles of heat treatment after tin electroplating are used to promote the combination of the tin layer and the pins, improve connectivity and stability, ensure the connection quality between the tin layer and the pins, avoid tin migration and tin whisker growth problems in extreme environmental tests, prevent tin migration and whisker generation in extreme environments from causing short circuit failure between device pins, and improve the connection stability of the integrated circuit.
[0047] 2. In the present invention, by adding a crystal refiner to the electroplating solution, the grain structure of the electroplated tin layer can be effectively improved, the coating performance and quality can be improved, and the integrated circuit pins can have a denser pure tin coating structure, which is beneficial to improving the corrosion resistance, wear resistance and welding performance of the coating. By replacing the traditional tin-lead coating with a pure tin coating, the harm of lead in integrated circuit welding is avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The present invention is a flow chart of an integrated circuit pin welding tinning process. DETAILED DESCRIPTION
[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] Example 1
[0051] See also Figure 1 This embodiment provides a technical solution: a tinning process for integrated circuit pin welding, comprising the following steps:
[0052] Step 1: Clamp the integrated circuit pins and clean the integrated circuit pins to remove impurities and oil stains on the surface;
[0053] The cleaning process of the integrated circuit pins includes the following steps:
[0054] 11) Use chlorine-free detergent and deionized water in an ultrasonic cleaning machine and set the corresponding parameters;
[0055] 12) Place the integrated circuit pins in an ultrasonic cleaning machine and start the equipment for cleaning to remove dirt attached to the surface of the integrated circuit pins;
[0056] 13) After cleaning, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the detergent residue is completely removed;
[0057] 14) Place the cleaned integrated circuit pins into a drying device for drying;
[0058] Step 2: pre-treating the cleaned integrated circuit pins before electroplating, including electrolytic deburring, deoxidation and activation treatment;
[0059] The pre-plating pretreatment of the cleaned integrated circuit pins includes the following steps:
[0060] 21) Place the cleaned integrated circuit pins into the electrolytic bath, keeping the pins from touching each other;
[0061] 22) Filling the electrolyte to start the electrolytic deburring equipment, applying current and voltage to perform deburring treatment;
[0062] 23) placing the deburred integrated circuit pins into a deoxidation device for deoxidation treatment;
[0063] 24) placing the deoxidized integrated circuit pins into an activation tank for activation treatment;
[0064] 25) After the pretreatment is completed, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the treatment liquid is completely removed;
[0065] Step 3: Immerse the cleaned and pre-treated integrated circuit pins in an electroplating tank containing a crystal refiner, and then perform an electroplating tin operation on the integrated circuit pins, and apply an electric current to deposit tin salt on the surface of the pins to form a uniform tin layer;
[0066] The integrated circuit pin electroplating tinning operation includes the following steps:
[0067] 31) Prepare the electroplating tinning equipment and install the integrated circuit pins to be electroplated in the electroplating fixture or tank to ensure that the pins do not touch each other;
[0068] 32) adjusting the temperature and concentration of the plating solution in the plating tank, adding a crystal refiner to the plating solution, and fully mixing the crystal refiner with the plating solution; wherein the main components of the crystal refiner are: a mixture of long-chain compounds capable of improving cathode polarization and a trace amount of lanthanide metal complex salt;
[0069] 33) Place the installed pin fixture into the electroplating tank and allow the pins to be completely immersed in the electroplating solution;
[0070] 34) Set the current density and electroplating time, start the electroplating equipment, and start the electroplating process. The current density is 10A / dm 2 , the electroplating time is 40s;
[0071] Step 4: After the electroplating is completed, the integrated circuit pins are taken out for cleaning and washing to remove impurities and solvents remaining in the electroplating solution;
[0072] The cleaning and washing process is as follows: placing the electroplated integrated circuit pins into a cleaning tank or cleaning equipment; soaking and washing the pins with a cleaning agent for a period of time to remove the dirt and impurities remaining in the electroplating solution; using a neutralizing agent for neutralization after washing; and finally washing the cleaned integrated circuit pins with clean water to remove the residue of the cleaning agent.
[0073] Step 5: Dry the processed integrated circuit pins to ensure that the surface is clean and free of water marks; the drying process adopts a hot air drying process, and the specific process includes the following steps:
[0074] 51) placing the tinned integrated circuit pins into a drying oven for drying;
[0075] 52) Adjust the drying box temperature to 50-80 degrees Celsius, the drying time to 15-50 minutes, and the wind speed to 1-2 m / s;
[0076] 53) After the drying process is completed, the integrated circuit pins are naturally cooled to room temperature;
[0077] Step 6: Heat-treat the integrated circuit pins with tin to ensure that the tin crystals are rearranged without melting the tin, and perform three consecutive cycles of heat treatment; wherein the heat treatment includes the following steps:
[0078] 61) placing the tinned integrated circuit pins into a heat treatment furnace for preheating at a temperature of 160-218° C.;
[0079] 62) Setting the heat treatment temperature and time of the heat treatment furnace for heat treatment;
[0080] 63) After the heat treatment is completed, the integrated circuit pins are cooled naturally;
[0081] 64) Repeat the above steps three times to complete the heat treatment;
[0082] Step 7: After the heat treatment is completed, the integrated circuit pins are tested and packaged after passing the test.
[0083] Example 2
[0084] See also Figure 1 This embodiment provides a technical solution: a tinning process for integrated circuit pin welding, comprising the following steps:
[0085] Step 1: Clamp the integrated circuit pins and clean the integrated circuit pins to remove impurities and oil stains on the surface;
[0086] The cleaning process of the integrated circuit pins includes the following steps:
[0087] 11) Use chlorine-free detergent and deionized water in an ultrasonic cleaning machine and set the corresponding parameters;
[0088] 12) Place the integrated circuit pins in an ultrasonic cleaning machine and start the equipment for cleaning to remove dirt attached to the surface of the integrated circuit pins;
[0089] 13) After cleaning, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the detergent residue is completely removed;
[0090] 14) Place the cleaned integrated circuit pins into a drying device for drying;
[0091] Step 2: pre-treating the cleaned integrated circuit pins before electroplating, including electrolytic deburring, deoxidation and activation treatment;
[0092] The pre-plating pretreatment of the cleaned integrated circuit pins includes the following steps:
[0093] 21) Place the cleaned integrated circuit pins into the electrolytic bath, keeping the pins from touching each other;
[0094] 22) Filling the electrolyte to start the electrolytic deburring equipment, applying current and voltage to perform deburring treatment;
[0095] 23) placing the deburred integrated circuit pins into a deoxidation device for deoxidation treatment;
[0096] 24) placing the deoxidized integrated circuit pins into an activation tank for activation treatment;
[0097] 25) After the pretreatment is completed, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the treatment liquid is completely removed;
[0098] Step 3: Immerse the cleaned and pre-treated integrated circuit pins in an electroplating tank containing a crystal refiner, and then perform an electroplating tin operation on the integrated circuit pins, and apply an electric current to deposit tin salt on the surface of the pins to form a uniform tin layer;
[0099] The integrated circuit pin electroplating tinning operation includes the following steps:
[0100] 31) Prepare the electroplating tinning equipment and install the integrated circuit pins to be electroplated in the electroplating fixture or tank to ensure that the pins do not touch each other;
[0101] 32) adjusting the temperature and concentration of the plating solution in the plating tank, adding a crystal refiner to the plating solution, and fully mixing the crystal refiner with the plating solution; wherein the main components of the crystal refiner are: a mixture of long-chain compounds capable of improving cathode polarization and a trace amount of lanthanide metal complex salt;
[0102] 33) Place the installed pin fixture into the electroplating tank and allow the pins to be completely immersed in the electroplating solution;
[0103] 34) Set the current density and electroplating time, start the electroplating equipment, and start the electroplating process. The current density is 15A / dm 2 , the electroplating time is 60s;
[0104] Step 4: After the electroplating is completed, the integrated circuit pins are taken out for cleaning and washing to remove impurities and solvents remaining in the electroplating solution;
[0105] The cleaning and washing process is as follows: placing the electroplated integrated circuit pins into a cleaning tank or cleaning equipment; soaking and washing the pins with a cleaning agent for a period of time to remove the dirt and impurities remaining in the electroplating solution; using a neutralizing agent for neutralization after washing; and finally washing the cleaned integrated circuit pins with clean water to remove the residue of the cleaning agent.
[0106] Step 5: Dry the processed integrated circuit pins to ensure that the surface is clean and free of water marks; the drying process adopts a hot air drying process, and the specific process includes the following steps:
[0107] 51) placing the tinned integrated circuit pins into a drying oven for drying;
[0108] 52) Adjust the drying box temperature to 50-80 degrees Celsius, the drying time to 15-50 minutes, and the wind speed to 1-2 m / s;
[0109] 53) After the drying process is completed, the integrated circuit pins are naturally cooled to room temperature;
[0110] Step 6: Heat-treat the integrated circuit pins with tin to ensure that the tin crystals are rearranged without melting the tin, and perform three consecutive cycles of heat treatment; wherein the heat treatment includes the following steps:
[0111] 61) placing the tinned integrated circuit pins into a heat treatment furnace for preheating at a temperature of 160-218° C.;
[0112] 62) Setting the heat treatment temperature and time of the heat treatment furnace for heat treatment;
[0113] 63) After the heat treatment is completed, the integrated circuit pins are cooled naturally;
[0114] 64) Repeat the above steps three times to complete the heat treatment;
[0115] Step 7: After the heat treatment is completed, the integrated circuit pins are tested and packaged after passing the test.
[0116] Example 3
[0117] See also Figure 1 This embodiment provides a technical solution: a tinning process for integrated circuit pin welding, comprising the following steps:
[0118] Step 1: Clamp the integrated circuit pins and clean the integrated circuit pins to remove impurities and oil stains on the surface;
[0119] The cleaning process of the integrated circuit pins includes the following steps:
[0120] 11) Use chlorine-free detergent and deionized water in an ultrasonic cleaning machine and set the corresponding parameters;
[0121] 12) Place the integrated circuit pins in an ultrasonic cleaning machine and start the equipment for cleaning to remove dirt attached to the surface of the integrated circuit pins;
[0122] 13) After cleaning, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the detergent residue is completely removed;
[0123] 14) Place the cleaned integrated circuit pins into a drying device for drying;
[0124] Step 2: pre-treating the cleaned integrated circuit pins before electroplating, including electrolytic deburring, deoxidation and activation treatment;
[0125] The pre-plating pretreatment of the cleaned integrated circuit pins includes the following steps:
[0126] 21) Place the cleaned integrated circuit pins into the electrolytic bath, keeping the pins from touching each other;
[0127] 22) Filling the electrolyte to start the electrolytic deburring equipment, applying current and voltage to perform deburring treatment;
[0128] 23) placing the deburred integrated circuit pins into a deoxidation device for deoxidation treatment;
[0129] 24) placing the deoxidized integrated circuit pins into an activation tank for activation treatment;
[0130] 25) After the pretreatment is completed, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the treatment liquid is completely removed;
[0131] Step 3: Immerse the cleaned and pre-treated integrated circuit pins in an electroplating tank containing a crystal refiner, and then perform an electroplating tin operation on the integrated circuit pins, and apply an electric current to deposit tin salt on the surface of the pins to form a uniform tin layer;
[0132] The integrated circuit pin electroplating tinning operation includes the following steps:
[0133] 31) Prepare the electroplating tinning equipment and install the integrated circuit pins to be electroplated in the electroplating fixture or tank to ensure that the pins do not touch each other;
[0134] 32) adjusting the temperature and concentration of the plating solution in the plating tank, adding a crystal refiner to the plating solution, and fully mixing the crystal refiner with the plating solution; wherein the main components of the crystal refiner are: a mixture of long-chain compounds capable of improving cathode polarization and a trace amount of lanthanide metal complex salt;
[0135] 33) Place the installed pin fixture into the electroplating tank and allow the pins to be completely immersed in the electroplating solution;
[0136] 34) Set the current density and electroplating time, start the electroplating equipment, and start the electroplating process. The current density is 20A / dm 2 , the electroplating time is 80s;
[0137] Step 4: After the electroplating is completed, the integrated circuit pins are taken out for cleaning and washing to remove impurities and solvents remaining in the electroplating solution;
[0138] The cleaning and washing process is as follows: placing the electroplated integrated circuit pins into a cleaning tank or cleaning equipment; soaking and washing the pins with a cleaning agent for a period of time to remove the dirt and impurities remaining in the electroplating solution; using a neutralizing agent for neutralization after washing; and finally washing the cleaned integrated circuit pins with clean water to remove the residue of the cleaning agent.
[0139] Step 5: Dry the processed integrated circuit pins to ensure that the surface is clean and free of water marks; the drying process adopts a hot air drying process, and the specific process includes the following steps:
[0140] 51) placing the tinned integrated circuit pins into a drying oven for drying;
[0141] 52) Adjust the drying box temperature to 50-80 degrees Celsius, the drying time to 15-50 minutes, and the wind speed to 1-2 m / s;
[0142] 53) After the drying process is completed, the integrated circuit pins are naturally cooled to room temperature;
[0143] Step 6: Heat-treat the integrated circuit pins with tin to ensure that the tin crystals are rearranged without melting the tin, and perform three consecutive cycles of heat treatment; wherein the heat treatment includes the following steps:
[0144] 61) placing the tinned integrated circuit pins into a heat treatment furnace for preheating at a temperature of 160-218° C.;
[0145] 62) Setting the heat treatment temperature and time of the heat treatment furnace for heat treatment;
[0146] 63) After the heat treatment is completed, the integrated circuit pins are cooled naturally;
[0147] 64) Repeat the above steps three times to complete the heat treatment;
[0148] Step 7: After the heat treatment is completed, the integrated circuit pins are tested and packaged after passing the test.
[0149] Comparative Example 1
[0150] The tin plating process for integrated circuit pin welding provided in this embodiment is substantially the same as that in Embodiment 1, with the main difference being that in step three, no crystal refiner is added to the plating solution in the plating tank.
[0151] Comparative Example 2
[0152] The tin plating process for integrated circuit pin welding provided in this embodiment is substantially the same as that in embodiment 1, with the main difference being that the integrated circuit pin is not subjected to tin heat treatment after the electroplating is completed.
[0153] Process test
[0154] The electroplating performance test was performed on the tin-plated pins of the integrated circuit prepared in Examples 1-3 and Comparative Examples 1-2 respectively. The electroplating test requirements are: high temperature, high humidity (full steam) and high pressure, and the relevant data are recorded in Table 1;
[0155] Table 1: Test data record table
[0156]
[0157] It can be seen from Table 1 that, compared with the comparative example, the tin-plated pins of the integrated circuits prepared in Examples 1-4 did not have tin whisker growth under the test environment of high temperature, high humidity and high pressure, and had better performance in terms of solderability, and the low thermal expansion coefficient ensured the welding quality; good tin whisker length can ensure good welding connection, that is, during welding, the tin whisker can completely cover the welding area to achieve reliable welding connection; good solderability means that the surface of the tin-plated pin can easily form a uniform welding contact with the solder, which is beneficial to the wetting and diffusion of the solder during the welding process, thereby achieving a good welding contact area and welding quality; the grain size of the coating affects the uniformity and crystallinity of the tin-plated layer, and a smaller grain size usually means a denser coating structure, which is beneficial to improving the corrosion resistance, wear resistance and welding performance of the coating; a lower thermal expansion coefficient can avoid thermal stress caused by temperature changes, thereby reducing stress concentration in the welding area and improving the reliability of the welding connection.
[0158] In the present invention, by adding a crystal refiner to the electroplating solution, the grain structure of the electroplated tin layer can be effectively improved, the performance and quality of the plating layer can be improved, and after electroplating pure tin, three cycles of heat treatment are used to help promote the combination of the tin layer and the pins, improve connectivity and stability, ensure the connection quality between the tin layer and the pins, avoid tin migration and tin whisker growth problems in extreme environmental tests, and prevent tin migration and whisker generation in extreme environments from causing short circuit failure between device pins.
[0159] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A tinning process for integrated circuit pin welding, characterized in that: The following steps are involved: S1. Clamp the integrated circuit pins and load them, clean the integrated circuit pins, and remove impurities and oil stains on the surface; S2, pre-treatment of the cleaned integrated circuit pins before electroplating, including electrolytic deburring, deoxidation and activation treatment; S3, immersing the cleaned and pretreated integrated circuit pins in an electroplating tank containing a crystal refiner, and then performing an electrotin plating operation on the integrated circuit pins, and applying an electric current to deposit tin salt on the surface of the pins to form a uniform tin layer; S4, after the electroplating is completed, the integrated circuit pins are taken out for cleaning and washing to remove impurities and solvents remaining in the electroplating solution; S5. Dry the processed integrated circuit pins to ensure that the surface is clean and free of water marks; S6, heat-treating the integrated circuit pins with tin to ensure that the tin crystals are rearranged without melting the tin, and performing three consecutive cycles of heat treatment; S7. After the heat treatment is completed, the integrated circuit pins are tested and packaged after passing the test.
2. The integrated circuit pin soldering tinning process according to claim 1, characterized in that: In step S1, the cleaning process of the integrated circuit pins includes the following steps: S11. Use chlorine-free detergent and deionized water to put into ultrasonic cleaning machine and set corresponding parameters; S12, placing the integrated circuit pins into an ultrasonic cleaning machine, starting the equipment for cleaning, and removing dirt attached to the surface of the integrated circuit pins; S13. After cleaning, remove the integrated circuit pins and rinse them thoroughly with clean water to ensure that the detergent residue is completely removed; S14, placing the cleaned integrated circuit pins into a drying device for drying.
3. The tinning process for integrated circuit pin welding according to claim 1, characterized in that: In step S2, the pre-plating pretreatment of the cleaned integrated circuit pins includes the following steps: S21, placing the cleaned integrated circuit pins into an electrolytic bath, keeping the pins from contacting each other; S22, filling electrolyte to start the electrolytic deburring equipment, applying current and voltage to perform deburring processing; S23, placing the deburred integrated circuit pins into a deoxidation device for deoxidation treatment; S24, placing the deoxidized integrated circuit pins into an activation tank for activation treatment; S25. After the pretreatment is completed, the integrated circuit pins are taken out and rinsed thoroughly with clean water to ensure that the treatment liquid is completely removed.
4. The integrated circuit pin soldering tinning process according to claim 1, characterized in that: In step S3, the integrated circuit pin electrotinning operation includes the following steps: S31, prepare the electroplating tinning equipment, install the integrated circuit pins to be electroplated in the electroplating fixture or tank, and ensure that the pins do not contact each other; S32, adjusting the temperature and concentration of the electroplating solution in the electroplating tank, adding a crystallization refiner into the electroplating solution, and fully mixing the crystallization refiner with the electroplating solution; S33, placing the installed pin fixture into the electroplating tank, allowing the pin to be completely immersed in the electroplating solution; S34, setting the current density and electroplating time, starting the electroplating equipment, and starting the electroplating process.
5. The tinning process for integrated circuit pin welding according to claim 4, characterized in that: In step S34, the current density is 10-20A / dm 2 , the electroplating time is 40-80s.
6. The integrated circuit pin soldering tinning process according to claim 1, characterized in that: In step S4, the step of removing the integrated circuit pins for cleaning and washing includes the following steps: S41, placing the electroplated integrated circuit pins into a cleaning tank or cleaning equipment; S42, using a cleaning agent to soak and clean the pins for a period of time to remove dirt and impurities remaining in the electroplating solution; S43, after cleaning, using a neutralizing agent for neutralization treatment; S44. Finally, the cleaned integrated circuit pins are washed with clean water to remove the residue of the cleaning agent.
7. The integrated circuit pin soldering tinning process according to claim 1, characterized in that: In step S5, the drying process adopts a hot air drying process, and the specific process includes the following steps: S51, placing the tinned integrated circuit pins into a drying oven for drying; S52, adjust the drying box temperature to 50-80 degrees Celsius, the drying time to 15-50 minutes, and the wind speed to 1-2 m / s; S53. After the drying process is completed, the integrated circuit pins are naturally cooled to room temperature.
8. The integrated circuit pin soldering tinning process according to claim 1, characterized in that: In step S6, the heat treatment comprises the following steps: S61, placing the tin-plated integrated circuit pins into a heat treatment furnace for preheating; S62, setting the heat treatment temperature and time of the heat treatment furnace to perform heat treatment; S63, after the heat treatment is completed, the integrated circuit pins are naturally cooled; S64, repeat steps S61-S63 three times to complete the heat treatment.
9. The integrated circuit pin soldering tinning process according to claim 8, characterized in that: In step S61, the preheating temperature is 160-218°C.