Production method of durable high-non-ironing high-shape-retention woven fabric

Through the low-tension merceration and tidal cross-linking and super feeding process, a mesh structure is formed, which solves the problems of shrinkage and wrinkle after washing of pure cotton fabrics, and realizes the efficient production of high-iron and high-type woven fabrics, which improves the fabric Anti-wrinkle properties and value for taking.

CN119041072AInactive Publication Date: 2024-11-29LUTAI TEXTILE

Patent Information

Application Number
CN202411517016.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology is difficult to meet the needs of high-iron and high-type woven fabrics. Pure cotton fabrics shrink greatly after washing and are prone to wrinkles. The existing methods cannot effectively improve wrinkle resistance, especially the application scope for strip fabrics is narrow.

Method used

The low-tension merceration and tidal cross-linking high-super feeding process is adopted, and the elastic lifting agent and resin additive are processed together to form a mesh structure, which reduces the pre-shrinkage process, improves the meridian elasticity and wrinkle recovery angle of the fabric, and reduces the difficulty of sewing.

Benefits of technology

The fabric is high-iron-iron and high-type maintenance, and the flatness after washing is increased by 0.1 level, the wrinkle recovery angle is increased by 10%, and the meridian elasticity is increased by 1%, which improves the use value and Q-elastic feel of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of textile dyeing and finishing, and particularly relates to a production method of a durable high-non-ironing high-shape-retention woven fabric. The method sequentially comprises the following working procedures of fabric texture design, singeing, desizing, mercerizing, drying, liquid ammonia treatment, pretreatment, moist crosslinking resin padding, constant-temperature stacking, primary washing, secondary washing and tentering. Wherein the yarn count of the fabric is 30-40, the warp tightness of the fabric is 67-72%, the weft tightness of the fabric is 45%, the total tightness of the fabric is 82-85%, and the twist coefficient of the fabric is 245-470. The fabric is highly shaped and high in flatness, and the wrinkle recovery angle can reach 85% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile dyeing and finishing, and particularly relates to a method for producing a durable, highly wrinkle-free and high-shape-retaining woven fabric. Background Art

[0002] Pure cotton woven fabrics have good moisture absorption and breathability, and are soft to the touch and comfortable to wear, so they are popular in the market. However, pure cotton fabrics shrink a lot and wrinkle easily after washing, which seriously affects the wearing experience. Therefore, it is particularly important to improve the wrinkle resistance of the fabric.

[0003] Chinese invention patent publication number CN107938219A introduces a high-grade wrinkle-free finishing method for deep black pure cotton fabric, but its scope of application is relatively narrow and cannot meet customers' demand for striped fabrics.

[0004] Chinese invention patent publication number CN103541103A improves the anti-wrinkle effect by changing the conventional fabric structure specifications and dyeing depth. Without resin finishing, the fabric has a flatness of about 3.0 after washing and a wrinkle recovery angle of about 70%, which cannot meet customer demand for high-ironing and high-shape retention products. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for producing a durable, highly wrinkle-free and high-shape-retention woven fabric. The fabric of the present invention has high shape retention, high flatness, and a wrinkle recovery angle of more than 85%.

[0006] The production method of the durable, high-ironing-free and high-shape-retention woven fabric of the present invention comprises the following steps in sequence: fabric organization design → singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking impregnation with resin → constant temperature stacking → primary water washing → secondary water washing → stentering; Among them, the fabric yarn count is 30~40, the warp tightness of the fabric is 67~72%, the weft tightness is 45%, the total tightness is 82~85%, and the twist coefficient is 245~470.

[0007] Preferably, in the singeing process, the burner position is selected as opposite burning, the flame intensity is 12-14 mbar, and the vehicle speed is 100 m / min.

[0008] Preferably, in the desizing process, the steamer temperature is 95-98°C, the stacking time is 10-15min, the vehicle speed is 80-100m / min, the washing temperature is 90-95°C, and the desizing solution includes: 10-20g / L high-temperature desizing enzyme, 5g / L penetrant, and 15-20g / L refining agent; the high-temperature desizing enzyme is preferably DS-HT from Zibo Lurui Fine Chemical Co., Ltd., the refining agent is preferably XC-J from Qingdao Collaborative Chemical Co., Ltd., and the penetrant is preferably WR-03 from Qingdao Ounosi Industry and Trade Co., Ltd.

[0009] Preferably, in the mercerizing process, the alkali concentration is 18-20 degrees Baume, the needle plate tension is 80-100N, the vehicle speed is 25-30m / min, the alkali temperature is 25-30°C, the washing tank temperature is 75-80°C, and the fabric pH value is 6-7.

[0010] Preferably, in the drying process, the vehicle speed is 50-70 m / min and the drying room temperature is 100-110°C.

[0011] Preferably, in the liquid ammonia process, the vehicle speed is 30-45 m / min, the water washing temperature is room temperature, and the pH value is 5.5-7.0.

[0012] Preferably, the pretreatment process is carried out on a tenter, and the additives and dosages used are: acid-base stabilizer PH-X: 2-3 g / L, water-absorbing softener SEH-02: 20-30 g / L; the tenter drying room temperature is 100-110°C, and the speed is 60-70 m / min. Among them, PH-X and SEH-02 are produced by Zibo Lurui Fine Chemical Co., Ltd.

[0013] Preferably, the moisture cross-linking and impregnation resin process is carried out on a tenter frame, the drying room temperature is 70-90°C, the cloth drop temperature and humidity are 38-40°C and 6.5-8% respectively, the vehicle speed is 35-40 m / min, and the overfeed is 3-5%.

[0014] Preferably, the additives and dosages of the moisture cross-linking padding resin process are: resin Z-RH: 200~240g / L, catalyst UMP: 100~120g / L, fiber protector SF-P: 20~40g / L, hydrophilic softener SEH-02: 20~30g / L, elasticity enhancer UR: 20~30g / L. Among them, Z-RH and UMP are produced by Huntsman Chemical Trading (Shanghai) Co., Ltd., SF-P and SEH-02 are produced by Zibo Lurui Fine Chemical Co., Ltd., and UR is a polyether polyurethane polymer UR produced by Qingdao Xianda Fine Chemical Co., Ltd.

[0015] Preferably, in the constant temperature stacking process, the temperature is 38-40°C, the humidity is 7-8%, and the stacking is 20-24 hours.

[0016] Preferably, the primary washing and the secondary washing are both carried out on a washing machine, which has 8 washing tanks. The primary washing temperature is 65-70°C, soda ash is added to the first washing tank, the addition amount is 15-20g / L, and the vehicle speed is 30-35m / min; the secondary washing temperature is 40-50°C, the vehicle speed is 50-60m / min, the fabric pH value is 5-7, and the formaldehyde content is controlled within 40ppm.

[0017] Preferably, the additives and dosages used in the tentering process are: acid-base stabilizer PH-X: 2-3 g / L, softener SMI-60: 20-40 g / L, formaldehyde scavenger FDS: 20-30 g / L, overfeed 2-5%, weft straightening, and cloth humidity 4-5%. PH-X, SMI-60 and FDS are all produced by Zibo Lurui Fine Chemical Co., Ltd.

[0018] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses low-tension mercerization and moisture-crosslinking high superfeeding to shape the warp yarn under low-tension conditions, reduce the pre-shrinkage process, shorten the process flow, increase the warp elasticity of the fabric by more than 1%, and increase the wrinkle recovery angle by up to 10%, giving the fabric more wearing value and reducing the difficulty of sewing; 2. The present invention processes the elasticity enhancer and the resin additive in the same bath. The resin connects the adjacent macromolecular chains in the fiber to form a network structure. The elasticity of the fabric is improved after deformation by external force. No adhesive needs to be added. The effect is long-lasting and the operation is simple. The wrinkle recovery angle and elastic feel of the fabric are improved. DETAILED DESCRIPTION

[0019] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0020] All raw materials used in the examples are commercially available unless otherwise specified, including: High temperature desizing enzyme DS-HT, Zibo Lurui Fine Chemical Co., Ltd.; Refining agent XC-J, Qingdao Collaborative Chemical Co., Ltd.; Penetrant WR-03, Qingdao Onosi Industry and Trade Co., Ltd.; Acid-base stabilizer PH-X, Zibo Lurui Fine Chemical Co., Ltd.; Water-absorbent softener SEH-02, Zibo Lurui Fine Chemical Co., Ltd.; Resin Z-RH, Huntsman Chemical Trading (Shanghai) Co., Ltd.; Catalyst UMP, Huntsman Chemical Trading (Shanghai) Co., Ltd.; Fiber protective agent SF-P, Zibo Lurui Fine Chemical Co., Ltd.; Elasticity enhancer UR, Qingdao Xianda Fine Chemical Co., Ltd.; Softener SMI-60, Zibo Lurui Fine Chemical Co., Ltd.; Formaldehyde scavenger FDS, Zibo Lurui Fine Chemical Co., Ltd.; Resin AMC, Qingdao Collaborative Chemical Co., Ltd.; Catalyst LRMC, Zibo Lurui Fine Chemical Co., Ltd.

[0021] Example 1 The sample is a herringbone twill fabric with white yarn in the warp and blue yarn in the weft. The warp yarn is CPT40, the weft yarn is CPT30, the warp density is 130 strands / inch, the weft density is 70 strands / inch, the warp tightness is 72%, the weft tightness is 45%, and the total fabric tightness is 85%; the warp twist coefficient is 330, and the weft twist coefficient is 470.

[0022] The specific implementation steps are: The process is as follows: singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking impregnation with resin → constant temperature stacking → primary water washing → secondary water washing → stentering.

[0023] Singeing and desizing process: carried out on a combined machine, singeing is carried out by counter-singing, the flame intensity is 14mbar, the speed is 100m / min, the fabric is singed on both sides, first the back side and then the front side; desizing is carried out by enzyme desizing, the steamer temperature is 95℃, the stacking time is 10min, the speed is 80m / min, the washing temperature is 95℃, and the desizing liquid includes: high temperature desizing enzyme DS-HT at a dosage of 10g / L, penetrant WR-03: 5g / L, and refining agent XC-J: 15g / L.

[0024] Mercerizing process: alkali concentration 18 degrees Baume, needle plate tension 80N, machine speed 25m / min, alkali temperature 25℃, washing tank temperature 75℃, fabric pH 6.0.

[0025] Drying process: vehicle speed 50m / min, drying room temperature 100℃.

[0026] Liquid ammonia process: vehicle speed is 30m / min, water washing temperature is room temperature, pH value is 5.5.

[0027] Pretreatment process: carried out on a tenter frame, acid-base stabilizer PH-X: 2g / L, water-absorbing softener SEH-02: 30g / L, tenter frame drying room temperature of 100°C, speed of 60m / min.

[0028] Moisture cross-linking padding resin process: carried out on a tenter frame, the drying room temperature is 70°C, the cloth temperature and humidity are controlled at 38°C and 6.5% respectively, the speed is 35m / min, and the overfeed is 3%. The additives and dosages of the moisture cross-linking padding resin process are: resin Z-RH: 220g / L, catalyst UMP: 110g / L, fiber protection agent SF-P: 40g / L, hydrophilic softener SEH-02: 30g / L, elasticity enhancer UR: 20g / L.

[0029] Constant temperature stacking: temperature 40℃, humidity 7%, stacking for 20h.

[0030] Washing process: Both the first and second washing are carried out on a washing machine. The washing machine has 8 washing tanks. The first washing temperature is 70°C. 15g / L of soda ash is added to the first washing tank. The vehicle speed is 30m / min. The second washing temperature is 50°C, the pH value of the fabric is 5, the formaldehyde content is controlled at 30ppm, the vehicle speed is 60m / min, and the pH value of the fabric is 5.5.

[0031] Stretching process: acid-base stabilizer PH-X: 3g / L, softener SMI-60: 20g / L, formaldehyde scavenger FDS: 20g / L, overfeed 3%, weft straightening, cloth humidity 4%.

[0032] Example 2 The sample is pink positive and negative twill fabric, the warp yarn is CPT40, the weft yarn is CPT30, the warp density is 120 strands / inch, the weft density is 70 strands / inch, the warp tightness is 67%, the weft tightness is 45%, and the total fabric tightness is 82%; the warp twist coefficient is 330, and the weft twist coefficient is 470.

[0033] The specific implementation steps are: The process is as follows: singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking impregnation with resin → constant temperature stacking → primary water washing → secondary water washing → stentering.

[0034] Singeing and desizing process: carried out on a combined machine, with double burning, flame intensity of 12mbar, machine speed of 100m / min, and fabrics singed on both sides, first on the back and then on the front; desizing is carried out by enzyme desizing, steamer temperature of 98℃, stacking time of 15min, machine speed of 100m / min, washing temperature of 90℃, high temperature desizing enzyme DS-HT dosage of 20g / L, penetrant WR-03: 5g / L, refining agent XC-J: 20g / L.

[0035] Mercerizing process: alkali concentration 20 degrees Baume, needle plate tension 100N, machine speed 30m / min, alkali temperature 30℃, washing tank temperature 80℃, fabric pH value 7.

[0036] Drying process: vehicle speed 70m / min, drying room temperature 110℃.

[0037] Liquid ammonia process: vehicle speed is 45m / min, water washing temperature is room temperature, pH value is 7.

[0038] Pretreatment process: carried out on a tenter frame, acid-base stabilizer PH-X: 3g / L, water-absorbing softener SEH-02: 20g / L, tenter frame drying room temperature of 110°C, speed of 70m / min.

[0039] Moisture cross-linking padding resin process: carried out on a tenter frame, the drying room temperature is 90°C, the cloth temperature and humidity are controlled at 40°C and 7.5% respectively, the speed is 40m / min, and the overfeed is 5%. The additives and dosages of the moisture cross-linking padding resin process are: resin Z-RH: 240g / L, catalyst UMP: 120g / L, fiber protection agent SF-P: 30g / L, hydrophilic softener SEH-02: 20g / L, elasticity enhancer UR: 30g / L.

[0040] Constant temperature stacking: temperature 38℃, humidity 8%, stacking for 24h.

[0041] Washing process: Both the first and second washing are carried out on a washing machine. The washing machine has 8 washing tanks. The first washing temperature is 65°C. 20g / L of soda ash is added to the first washing tank. The vehicle speed is 35m / min. The second washing temperature is 40°C, the fabric pH value is 7, the formaldehyde content is controlled at 35ppm, and the vehicle speed is 50m / min.

[0042] Stretching process: acid-base stabilizer PH-X: 2g / L, softener SMI-60: 40g / L, formaldehyde scavenger FDS: 30g / L, overfeed 2%, weft straightening, cloth humidity 5%.

[0043] Example 3 The sample is a blue and white striped jacquard fabric, the warp yarn is CPT40, the weft yarn is CPT30, the warp density is 130 strands / inch, the weft density is 70 strands / inch, the warp tightness is 72%, the weft tightness is 45%, and the total fabric tightness is 85%; the warp twist coefficient is 245, and the weft twist coefficient is 380.

[0044] The specific implementation steps are: The process is as follows: singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking impregnation with resin → constant temperature stacking → primary water washing → secondary water washing → stentering.

[0045] Singeing and desizing process: carried out on a combined machine, with double burning adopted for singeing, flame intensity of 12mbar, machine speed of 100m / min, and fabrics singed on both sides, first on the back side and then on the front side; desizing adopts enzyme desizing method, steamer temperature of 96℃, stacking time of 12min, machine speed of 90m / min, washing temperature of 92℃, high temperature desizing enzyme DS-HT dosage of 20g / L, penetrant WR-03: 5g / L refining agent XC-J: 18g / L.

[0046] Mercerizing process: alkali concentration 18 degrees Baume, needle plate tension 95N, machine speed 28m / min, alkali temperature 28℃, washing tank temperature 78℃, fabric pH value 7.

[0047] Drying process: vehicle speed 60m / min, drying room temperature 110℃.

[0048] Liquid ammonia process: vehicle speed is 40m / min, water washing temperature is room temperature, pH value is 6.2.

[0049] Pretreatment process: carried out on a tenter frame, acid-base stabilizer PH-X: 2g / L, water-absorbing softener SEH-02: 20g / L, tenter frame drying room temperature of 105°C, speed of 70m / min.

[0050] Moisture cross-linking padding resin process: carried out on a tenter frame, the drying room temperature is 85°C, the cloth temperature and humidity are controlled at 39°C and 6% respectively, the speed is 38m / min, and the overfeed is 5%. The additives and dosages of the moisture cross-linking padding resin process are: resin Z-RH: 200g / L, catalyst UMP: 100g / L, fiber protection agent SF-P: 20g / L, hydrophilic softener SEH-02: 30g / L, elasticity enhancer UR: 30g / L.

[0051] Constant temperature stacking: temperature 40℃, humidity 7.5%, stacking for 22h.

[0052] Washing process: Both the first and second washing are carried out on a washing machine. The washing machine has 8 washing tanks. The first washing temperature is 70°C. 15g / L of soda ash is added to the first washing tank. The vehicle speed is 35m / min. The second washing temperature is 40°C, the fabric pH value is 6.8, the formaldehyde content is controlled at 35ppm, and the vehicle speed is 60m / min.

[0053] Stretching process: acid-base stabilizer PH-X: 2g / L, softener SMI-60: 30g / L, formaldehyde scavenger FDS: 30g / L, overfeed 5%, weft straightening, cloth humidity 5%.

[0054] Comparative Example 1 The sample is a herringbone twill fabric with white warp yarn and blue weft yarn interwoven. The warp yarn is CPT40, the weft yarn is CPT30, the warp density is 130 strands / inch, and the weft density is 70 strands / inch. The warp tightness is 72%, the weft tightness is 45%, and the total tightness of the fabric is 85%; the warp twist coefficient is 330, and the weft twist coefficient is 470. The specific implementation steps are: The process is as follows: singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking impregnation with resin → constant temperature stacking → primary water washing → secondary water washing → stentering.

[0055] Singeing and desizing process: It is carried out on a combined machine. Direct burning is used for singeing, the flame intensity is 12mbar, the speed is 95m / min, and the fabric is singed on both sides, first the back side and then the front side; desizing is carried out by enzyme desizing, and the dosage of high-temperature desizing enzyme DS-HT is 20g / L.

[0056] Mercerizing process: alkali concentration 20 degrees Baume, tension 220N, speed 30m / min, alkali temperature 30℃, washing tank temperature 75℃, pH value of woven fabric after mercerization is 6.5.

[0057] Liquid ammonia process: vehicle speed is 35m / min, water washing temperature is room temperature, pH value is 6.2.

[0058] Pretreatment process: carried out on a tenter frame, water-absorbing softener SEH-02: 30g / L, tenter frame drying room temperature of 100°C, speed of 55m / min.

[0059] The first pre-shrinkage: speed 40m / min, rubber blanket temperature 110℃, wool blanket temperature 80℃, pressing distance 12mm, warp shrinkage of fabric +0.5%.

[0060] Moisture cross-linking padding resin process: carried out on a tenter frame, the drying room temperature is 90°C, the cloth temperature and humidity are controlled at 38°C and 6.8% respectively. The additives and dosage are: resin AMC: 240g / L, catalyst LRMC: 120g / L, fiber protection agent SF-P: 30g / L, overfeed 3%.

[0061] Constant temperature stacking: temperature 40℃, humidity 7.5, stacking for 24h.

[0062] Washing process: Both the first and second washing are carried out on a washing machine. The washing machine has 8 washing tanks. The first washing temperature is 65°C. 20g / L of soda ash is added to the first washing tank. The vehicle speed is 40m / min. The second washing temperature is room temperature, the fabric pH value is 5.8, the formaldehyde content is controlled at 40ppm, and the vehicle speed is 60m / min.

[0063] Stretching process: acid-base stabilizer PH-X: 2g / L, softener SMI-60: 30g / L, formaldehyde scavenger FDS: 30g / L, overfeed 5%, weft straightening, cloth humidity 5%.

[0064] Second preshrinkage: machine speed 50m / min, rubber blanket temperature 100℃, wool blanket temperature 80℃, pressing distance 5mm.

[0065] Performance Testing The fabrics obtained in Examples 1 to 3 and Comparative Example 1 were subjected to performance tests, and the results are shown in Table 1. The smoothness of the appearance after washing was tested according to the JIS L1930 C4M standard, the wrinkle recovery angle was tested according to the JIS L1059-1 standard, and the warp / weft elasticity was tested according to the JIS L1096 standard. As can be seen from Table 1, the smoothness of the appearance after washing of the present invention is improved by more than 0.1 level compared with Comparative Example 1, the wrinkle recovery angle is improved by about 10%, and the warp elasticity is improved by more than 1%.

[0066] Table 1 Performance test table of Examples 1 to 3 and Comparative Example 1

Claims

1. A method for producing a durable, high-ironing and high-shape-retention woven fabric, characterized in that: The process includes the following steps: fabric organization design → singeing → desizing → mercerizing → drying → liquid ammonia → pretreatment → moisture cross-linking padding resin → constant temperature stacking → primary washing → secondary washing → stentering; Among them, the fabric yarn count is 30~40, the warp tightness of the fabric is 67~72%, the weft tightness is 45%, the total tightness is 82~85%, and the twist coefficient is 245~470.

2. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: In the mercerizing process, the alkali concentration is 18~20 degrees Baume, the needle plate tension is 80~100N, the machine speed is 25~30m / min, the alkali temperature is 25~30℃, the washing tank temperature is 75~80℃, and the fabric pH value is 6~7.

3. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: The pretreatment process is carried out on a stenter frame, and the additives and dosages used are: acid-base stabilizer PH-X: 2~3g / L, water-absorbing softener SEH-02: 20~30g / L; the drying room temperature of the stenter frame is 100~110℃, and the speed is 60~70m / min.

4. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: The moisture-crosslinked impregnation resin process is carried out on a tenter frame. The drying room temperature is 70~90℃, the cloth drop temperature and humidity are 38~40℃ and 6.5~8% respectively, the machine speed is 35~40m / min, and the overfeed is 3~5%.

5. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: The additives and dosage of the moisture cross-linking padding resin process are: resin Z-RH: 200~240g / L, catalyst UMP: 100~120g / L, fiber protective agent SF-P: 20~40g / L, hydrophilic softener SEH-02: 20~30g / L, elasticity enhancer UR: 20~30g / L.

6. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: In the constant temperature stacking process, the temperature is 38~40℃, the humidity is 7~8%, and the stacking time is 20~24h.

7. The method for producing a durable, high-ironing and high-shape-retention woven fabric according to claim 1, characterized in that: The additives and dosage used in the stentering process are: acid-base stabilizer PH-X: 2~3g / L, softener SMI-60: 20~40g / L, formaldehyde scavenger FDS: 20~30g / L, overfeeding 2~5%, weft straightening, and cloth humidity 4~5%.

Citation Information

Patent Citations

  • Processing method of non-ironing shirt fabric

    CN107299527A

  • Processing method for improving easy-care performance of moist crosslinking finishing yarn-dyed fabric

    CN108457082A

  • Warp-wise elastic tatting fabric and preparation method thereof

    CN111364146A

  • Processing technology for improving easy-care performance of linen fabric

    CN111793987A

  • Production process of formaldehyde-free moisture-state cross-linked fabric

    CN116791355A

Cited By

  • Processing method of super-comfortable natural anti-wrinkle fabric

    CN120625245A

  • Processing method of comfortable multifunctional high non-ironing yarn-dyed woven fabric

    CN121183488A