Coating for renovating plain brick wall and construction process thereof
Through imitation brick coating technology, combined with cement-based two-component combination and batch coating construction, the problems of wall cracks and water leakage during clean water brick wall repair are solved, the waterproof and reinforcement performance are improved, the coating life is extended, and the coating life is extended. The effect of restoring the old is achieved.
Patent Information
- Application Number
- CN202411042301.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
AI Technical Summary
The existing clean water brick wall repair technology cannot effectively solve the problems of wall cracks and water leakage, and the coating does not have enough waterproof and anti-aging protection for buildings.
The imitation brick coating includes imitation brick decorative mortar layer, caulking layer and color modification layer. It is constructed through two-component combination of cement-based base and batch coating in batches, combining the reinforcement of the base coating and the topcoat layer to enhance the coating and clean water bricks. The bonding strength and protective performance of the wall.
While renovating the old is still the same, it improves the waterproof, reinforcement and durability of the wall, extends the service life of the coating, and improves the overall coating effect through batch coating construction.
Smart Images

Figure CN119041644A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building repair, and in particular to a coating for renovating a plain brick wall and a construction process thereof. Background Art
[0002] The exposed brick wall is a brick wall that only needs to be grouted after the exterior wall is built. The exterior wall is no longer decorated, and the exposed bricks are required to have excellent qualities such as heat insulation, sound insulation, waterproof, frost resistance, durability, environmental protection and non-radioactivity. Because of its historical appearance, it is widely used in buildings such as schools, research institutes, and residential buildings. However, as the building ages, the surface of the exposed bricks begins to powder, grow mold, become dirty, and even crack. The cracks and peeling of the caulking material cause rainwater to seep in and the building to leak. For this reason, it is necessary to repair the old exposed brick walls.
[0003] The success or failure of the repair of exposed brick walls determines the continuation of the historical atmosphere and cultural life of the building. At present, the repair of exposed brick walls in China basically requires that the old be restored to its original state. The conventional practice is: 1. Clean the wall, remove the damaged bricks and caulking materials. Pickle the alkali-stained parts. 2. Repair the brick surface and use decorative mortar to mix the color of the brick for local repair. 3. Re-point the joints. 4. Apply silane water repellent on the surface. The advantage of this method is that it retains the appearance of the original wall to the greatest extent, but it cannot solve the problem of cracks and water leakage in the wall.
[0004] Patent CN109138482A provides a method for aging the plain bricks and Taishan bricks of the exterior walls of historical buildings, specifically a method for aging the plain bricks and Taishan bricks of the exterior walls of historical buildings that have been partially repaired and filled, by covering the surface of the bricks with a color matching agent coating, wherein the color matching agent coatings on the surfaces of two adjacent plain bricks or Taishan bricks are different colors, and the color matching agent coatings on the surface of the same plain brick or Taishan brick are the same color but different shades of color, the color matching agent coating used for the plain bricks is a mixture of mineral color powder and inorganic siloxane solution, or a mixture of acrylic polyurethane solution and inorganic siloxane solution; the color matching agent coating used for the Taishan bricks is a mixture of acrylic polyurethane solution and inorganic siloxane solution; the effect of restoring the exterior walls of historical buildings as if they were ancient can be achieved.
[0005] The above patent provides a solution for replicating the original building in appearance, but the coating cannot provide waterproof, anti-aging, or reinforcement protection for the original building. Summary of the invention
[0006] In view of the above problems, one of the objects of the present invention is to provide a coating for renovating exposed brick walls to solve the problems existing in the existing exposed brick wall repair; the second object of the present invention is to provide a construction process for renovating the coating for exposed brick walls to improve the overall coating effect.
[0007] One of the purposes of the present invention is achieved through the following technical solutions: A coating for renovating plain brick walls, comprising an imitation brick coating, the imitation brick coating comprising: an imitation brick decorative mortar layer and a caulking layer. The imitation brick decorative mortar layer is provided with a plurality of joints, and the joints are filled with the caulking layer. The imitation brick decorative mortar layer is formed by coating the imitation brick decorative mortar, the imitation brick decorative mortar comprising: a first liquid material and a first powder material, the ratio of the first liquid material to the first powder material is 1:2 to 1:4; wherein: the first liquid material comprises, by mass: 100 to 300 parts of water, 1 to 3 parts of preservative, 1 to 3 parts of cellulose, 1 to 3 parts of wetting agent, 1 to 3 parts of dispersant, 2 to 4 parts of defoaming agent, 50 to 100 parts of titanium dioxide, and 20 to 50 parts of fiber. , 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH adjuster, 1-3 parts of thickener, 20-50 parts of inorganic color paste; the first powder includes, by mass: 100-200 parts of heavy calcium, 200-300 parts of cement, 50-100 parts of gypsum, 200-400 parts of snow white, 1-3 parts of water reducer, 1-3 parts of anti-efflorescence aid, and 50-100 parts of closed-cap vitrified microspheres.
[0008] Preferably, the imitation brick coating further comprises a color correction layer coated on the surface of the imitation brick decorative mortar layer.
[0009] Preferably, the color correction layer is formed by coating a color correction agent, and the color correction agent includes: a second liquid and a second powder, and the ratio of the second liquid to the second powder is 1:0.5 to 1:2; wherein: the second liquid includes, by mass: 100 to 300 parts of water, 1 to 3 parts of preservatives, 1 to 3 parts of cellulose, 1 to 3 parts of wetting agents, 1 to 3 parts of dispersants, 2 to 4 parts of defoaming agents, 50 to 100 parts of titanium dioxide, 20 to 50 parts of fibers, 500 to 700 parts of acrylic emulsions, 20 to 40 parts of film-forming aids, 5 to 10 parts of ethylene glycol, 1 to 2 parts of pH regulators, 1 to 3 parts of thickeners, and 20 to 50 parts of inorganic color pastes; the second powder includes, by mass: 400 to 600 parts of heavy calcium, 200 to 300 parts of cement, 50 to 100 parts of gypsum, 1 to 3 parts of water reducers, and 1 to 3 parts of anti-efflorescence aids.
[0010] Preferably, the filling layer is formed by filling with a filling material, and the filling material includes: a third liquid and a third powder, and the ratio of the third liquid to the third powder is 1:3 to 1:5; wherein: the third liquid includes, by mass: 100 to 300 parts of water, 1 to 3 parts of preservatives, 1 to 3 parts of cellulose, 1 to 3 parts of wetting agents, 1 to 3 parts of dispersants, 2 to 4 parts of defoaming agents, 50 to 100 parts of titanium dioxide, 20 to 50 parts of fibers, 500 to 700 parts of acrylic emulsions, 20 to 40 parts of film-forming aids, 5 to 10 parts of ethylene glycol, 1 to 2 parts of pH regulators, 1 to 3 parts of thickeners, and 20 to 50 parts of inorganic color pastes; the third powder includes, by mass: 200 to 400 parts of cement, 600 to 800 parts of glass beads, 1 to 3 parts of water reducers, and 1 to 3 parts of anti-efflorescence aids.
[0011] Preferably, the gypsum is α-gypsum, and the fiber is aluminum silicate fiber.
[0012] Preferably, the coating used for renovating the exposed brick wall also includes a primer layer and a topcoat layer. The primer layer is applied to the surface of the exposed brick wall, the imitation brick coating layer is applied to the surface of the primer layer, and the topcoat layer is applied to the surface of the imitation brick coating layer. The present invention optimizes the coating matching, while improving the bonding strength between the coating and the exposed brick wall and the protective performance of the coating, thereby improving the service life of the coating.
[0013] Preferably, the base coat is formed by coating a reinforcing base coat, and the reinforcing base coat comprises, by mass, 100 to 200 parts of acrylic emulsion, 400 to 700 parts of water, 200 to 300 parts of inorganic potassium silicate, and 10 to 20 parts of a film-forming aid.
[0014] Preferably, the film-forming aid of the reinforced primer is ethylene glycol monobutyl ether.
[0015] Preferably, the topcoat layer is formed by coating with an isooctylsilane impregnating agent.
[0016] The second object of the present invention is achieved by the following technical solutions: A construction process for renovating a coating on a plain brick wall, wherein the imitation brick decorative mortar layer is constructed by batch coating in several steps, and the process is as follows: The first coat of imitation brick decorative mortar is used to level the joints of the exposed brick wall. The cracked and damaged joints need to be cleaned and then leveled; The second coat of imitation brick decorative mortar is applied to thicken the imitation brick decorative mortar layer, and masking paper is pre-embedded to outline the corresponding joints of the plain bricks. After the coating construction is completed, the masking paper is torn off to form joints on the imitation brick decorative mortar layer; The third coat of imitation brick decorative mortar is to shape the surface of the imitation brick decorative mortar layer to achieve the effect of imitating the surface appearance of plain bricks.
[0017] By adopting the above technical solution, the beneficial effects of the present invention are: 1. The imitation brick decorative mortar of the present invention adopts a cement-based two-component combination, so that the appearance of the imitation brick coating can be restored to its original state with consistent gloss, while also improving the waterproof, reinforcement and durability of the wall.
[0018] 2. In the construction process of the coating for renovating the plain brick wall of the present invention, the imitation brick decorative mortar layer is constructed by batch coating, and the overall coating effect is good and more firm and durable. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the construction of the imitation brick decorative mortar layer in batches according to an embodiment of the present invention. DETAILED DESCRIPTION
[0020] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0021] The embodiment of the present invention provides a coating for renovating a plain brick wall, comprising: a primer coating applied on the plain brick wall surface, an imitation brick coating applied on the surface of the primer coating, and a topcoat layer applied on the surface of the imitation brick coating.
[0022] The primer is obtained by applying a reinforcement primer to the surface of a plain brick wall.
[0023] Due to the micro-powdering of the surface of old clear water bricks, reinforcement treatment is required after the surface of the clear water bricks is cleaned. In addition, clear water bricks have many microporous structures, and mold grows in the moist parts 1 to 2 mm deep inside the bricks. If it is not killed, it will affect the strength of the clear water bricks in the long run. The commonly used primer is difficult to penetrate the interior and can only form a film on the surface. After drying, it is very easy to tear off in pieces. This embodiment uses an organic-inorganic composite coating, which has super permeability and reinforcement, and due to the high alkalinity of the inorganic components, it also has a certain killing effect on mold, achieving a sterilization and mildew prevention effect.
[0024] The reinforcement primer of this embodiment includes the following components in parts by weight: 100-200 parts of acrylic emulsion, 400-700 parts of water, 200-300 parts of inorganic potassium silicate, and 10-20 parts of film-forming aid.
[0025] Sources of some of the above raw materials: The acrylic emulsion selected is BASF's 7536 emulsion.
[0026] The inorganic potassium silicate used is TX-K48 type produced by Xi'an Tongxin Semiconductor Auxiliary Materials Co., Ltd.
[0027] The film-forming aid is ethylene glycol monobutyl ether.
[0028] Preparation method of reinforcement primer: put all components into disperser and stir at low speed.
[0029] The preparation examples in Table 1 were tested according to the tensile bonding strength test method of concrete interface agent in JC / T907-2018. The tensile bonding strength of each preparation example was ≥2.0Mpa, and the penetration depth on the red brick surface was 1 to 2mm. It can be seen that the base coating and the plain brick wall are firmly bonded.
[0030] Table 1
[0031] The imitation brick coating of the embodiment of the present invention needs to meet four requirements: First, the appearance must be consistent with the original clear water brick. Due to the sintering of clear water bricks, the gloss of the surface at different angles is less than 3°, and the color of each brick of the kiln-changed bricks is mottled. Second, the coating has a certain thickness, and the joint depth is consistent with the original clear water brick. The coating reinforces the original wall surface. Third, due to the high water content inside the original clear water brick, the coating must have water vapor permeability to facilitate the discharge of water, but no visible water can penetrate. Fourth, the water seepage parts of the old clear water bricks are mostly concentrated in the caulking, so the original caulking needs to be scraped and filled, and the appearance must be restored to be consistent with the original caulking.
[0032] In order to meet the requirements, the imitation brick coating of the embodiment of the present invention is realized by using imitation brick decorative mortar, color correcting agent and caulking material.
[0033] The imitation brick decorative mortar is applied on the surface of the base coating to form an imitation brick decorative mortar layer, and at the same time, a joint of a clear brick is opened on the imitation brick decorative mortar layer. A color correction agent is applied on the surface of the imitation brick decorative mortar layer to form a color correction layer. A joint filling material is applied in the joint of the imitation brick decorative mortar layer to form a joint filling layer.
[0034] The imitation brick decorative mortar of the embodiment of the present invention comprises a first liquid material and a first powder material, and the ratio of the two is 1:2 to 1:4, that is, 1 part of the first liquid material is mixed with 2 to 4 parts of the first powder material, preferably mixed in a ratio of 1:3.
[0035] The first liquid material has the following formula composition by mass: 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH adjuster, 1-3 parts of thickener and 20-50 parts of inorganic color paste.
[0036] Preparation method of the first liquid material: A. Add water, preservative, defoamer, wetting agent and dispersant into the disperser, and stir and disperse at a first speed; B. maintaining the first speed, adding cellulose, pH adjuster, fiber, and titanium dioxide in sequence and stirring and dispersing at the second speed; C. Set the speed of the disperser to the third speed, add acrylic emulsion, film-forming aid, ethylene glycol, and thickener in sequence for stirring and dispersing to obtain a liquid semi-finished product.
[0037] Among them, the first rotation speed is 400-500 rpm, the second rotation speed is 1200-1800 rpm, and the third rotation speed is 800-1000 rpm.
[0038] The first powder has the following formula composition by mass: 100-200 parts of heavy calcium, 200-300 parts of cement, 50-100 parts of gypsum, 200-400 parts of snow white (preferably including 100-200 parts of 20-40 mesh snow white and 100-200 parts of 40-80 mesh snow white), 1-3 parts of water reducing agent, 1-3 parts of anti-efflorescence additive, and 50-100 parts of closed-cap vitrified microspheres.
[0039] The first powder preparation method is: put all components into powder mixing equipment and mix them evenly.
[0040] The imitation brick decorative mortar of the embodiment of the present invention adopts the form of liquid-powder two-component, with cement, gypsum and acrylic emulsion as the main film-forming materials. Among them, acrylic emulsion provides color stability and durability. Cement and gypsum have the matte of inorganic coatings. Thick coating parts can also build strength without the need for complete evaporation of water. With the help of fibers, it will not crack due to drying shrinkage. During the drying process of gypsum, the coating color will appear mottled through the knife polishing and pressure construction, which is consistent with the appearance of plain bricks. In addition, the water activation process of cement and gypsum will naturally form a microporous structure, which is conducive to the discharge of water vapor. The microporous coating has waterproof and moisture permeability functions. The diameter of water vapor molecules is generally 4×10 -4 The diameter of a water droplet is usually 80 μm. The micropore size of the coating is generally 0.5 μm, so even the smallest raindrops cannot penetrate the micropores due to surface tension, while water vapor can pass freely.
[0041] The performance of the preparation examples in Table 2 were tested with reference to JG / T24-2018 "Synthetic resin sand-like exterior wall coating" and JC / T2090-2011 "Polymer cement waterproof slurry" Type II. The test results are shown in Table 3. It can be seen that the performance of the imitation brick decorative mortar has passed the standard requirements, and the bonding strength is much greater than the standard requirements.
[0042] Table 2
[0043] Table 3
[0044] The imitation brick decorative mortar layer of the embodiment of the present invention is constructed by batch coating in batches and formed by three times. The construction process is as follows: Figure 1 As shown. Among them, the first batch of imitation brick decorative mortar 3 is used to level the joints 2 of the clear brick wall 1. The cracked and damaged joints 2 need to be cleaned and then leveled. The second batch of imitation brick decorative mortar 3 is used to thicken the imitation brick decorative mortar layer, and the pre-embedded beauty paper 4 outlines the corresponding seams 5 of the clear bricks. The third batch of coating is to shape the surface of the imitation brick decorative mortar layer. Different processes can obtain different appearances. The specific process can be selected according to actual needs. This embodiment provides two processes. One is to rub the 20-40 mesh sand with an artistic washboard after the batch coating, so as to produce scratches and make horizontal lines imitating split bricks. The second is to paste a PE film on the surface after the batch coating, press the surface lightly, and cause the surface to be bumpy. After the paint film hardens, remove the PE film to obtain the bumpy antique brick effect. After the batch coating construction is completed, the masking paper 4 can be torn off to form a seam 5.
[0045] Due to the firing process of exposed bricks, some bricks will have different shades. Although gypsum has been added to the imitation brick decorative mortar to achieve this effect, if the color deviation is relatively large, it is necessary to use a color corrector to deepen it.
[0046] The color correcting agent of this embodiment includes: a second liquid material and a second powder material, and the ratio of the two is 1:0.5-1:2, that is, 1 part of the second liquid material is mixed with 0.5-2 parts of the second powder material, preferably mixed in a ratio of 1:1.
[0047] The second liquid material has the following formula composition by mass: 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH adjuster, 1-3 parts of thickener and 20-50 parts of inorganic color paste.
[0048] The second powder has the following formula composition by mass: 400-600 parts of heavy calcium, 200-300 parts of cement, 50-100 parts of gypsum, 1-3 parts of water reducing agent, and 1-3 parts of anti-efflorescence additive.
[0049] The method for using the color correcting agent is as follows: after the second liquid material and the second powder material are evenly stirred on site, the color correcting agent is applied with seaweed sponge or a brush.
[0050] The sealing material of this embodiment includes a third liquid material and a third powder material, and the ratio of the two is 1:3 to 1:5, that is, 1 part of the third liquid material is mixed with 3 to 5 parts of the third powder material, preferably mixed in a ratio of 1:4.
[0051] The third liquid material has the following formula composition by mass: 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH adjuster, 1-3 parts of thickener and 20-50 parts of inorganic color paste.
[0052] The third powder has the following formula composition by mass: 200-400 parts of cement, 600-800 parts of glass beads, 1-3 parts of water reducing agent, and 1-3 parts of anti-efflorescence additive.
[0053] Construction method of caulking material: After mixing the third liquid material and the third powder material evenly on site, use a caulking gun to squeeze and apply them to the joints, and use a grouting tool to level them.
[0054] The caulking material uses glass beads as the main filler. The surface of glass beads is smooth and does not absorb water. As a filler, it can have a high solid content, small shrinkage after drying, and high strength. Secondly, the surface of the grouting is smoother without wrinkles or scratches.
[0055] Sources of some of the above raw materials: The preservative used was Thor's EG-CLF.
[0056] The cellulose used is Dow's 15000PP.
[0057] The wetting agent used was Dow's BD109.
[0058] The dispersant used was BASF's 4140.
[0059] The defoaming agent used is Hemmings 7010.
[0060] The titanium dioxide used is R996 rutile titanium dioxide from Longmanguoli.
[0061] The acrylic emulsion used was 7382 from Badfu.
[0062] The film-forming aid is Runtai's dodecyl alcohol ester.
[0063] The pH regulator used was Dow's AMP-95.
[0064] The fiber is 1-2 mm long aluminum silicate fiber purchased from Lingshou County Shuolong Mineral Products Processing Plant.
[0065] The thickener used was Dow's TT-615.
[0066] Inorganic color paste is purchased from Clariant. The amount to be added is adjusted according to the color of the plain brick.
[0067] The specification of heavy calcium is 325 mesh, which is purchased from Jiangxi Guangyuan Chemical Co., Ltd.
[0068] Snow White is purchased from Guangxi Xinhuafa Powder Optimization Company.
[0069] The water reducing agent used is BASF's F10.
[0070] The cement used is Alborg's 42.5 ordinary Portland white cement.
[0071] The gypsum used was α gypsum, purchased from Wanhao Gypsum Industries Co., Ltd.
[0072] The anti-efflorescence additive is ERA-100 produced by Eletron.
[0073] The specifications of closed-end vitrified microspheres are 80-120 meshes, purchased from Zhengzhou Saint-Laite Hollow Microsphere New Materials Co., Ltd., which reduces the weight of the coating and increases the volume of the filler.
[0074] The specifications of glass beads are 80-120 mesh and are purchased from Guangdong Zhaotong Glass Plastic Technology Co., Ltd.
[0075] The imitation brick coating of the embodiment of the present invention has the following advantages: 1. The entire imitation brick coating adopts a cement-based two-component combination. While the appearance is restored to its original state and the gloss is consistent, it also improves the waterproof function, reinforcement and stain resistance of the wall.
[0076] 2. The imitation brick decorative mortar coating has various shapes and can achieve different brick textures according to different construction techniques.
[0077] 3. The caulking material uses glass beads and cement as the main fillers. The surface of glass beads is smooth and does not absorb water. As a filler, it can have a high solid content, small shrinkage after drying, and high strength. Secondly, the surface of the grouting is smoother without wrinkles or scratches.
[0078] 4. The combination of cement and gypsum can imitate the natural uneven color effect of plain bricks.
[0079] The topcoat layer of the embodiment of the present invention is formed by coating with an isooctylsilane impregnating agent, has good stain resistance, and can provide long-lasting protection for the imitation brick coating.
[0080] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes in form and details may be made to the present invention without departing from the spirit and scope of the invention as defined in the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A coating for renovating a plain brick wall, characterized in that: The imitation brick coating comprises: an imitation brick decorative mortar layer and a caulking layer; The imitation brick decorative mortar layer is provided with a plurality of joints, and the joints are filled with a caulking layer. The imitation brick decorative mortar layer is formed by coating the imitation brick decorative mortar, and the imitation brick decorative mortar comprises: a first liquid material and a first powder material, and the ratio of the first liquid material to the first powder material is 1:2 to 1:4; wherein: The first liquid material comprises, by mass, 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH regulator, 1-3 parts of thickener, and 20-50 parts of inorganic color paste; The first powder comprises, by mass, 100-200 parts of heavy calcium, 200-300 parts of cement, 50-100 parts of gypsum, 200-400 parts of snow white, 1-3 parts of water reducing agent, 1-3 parts of anti-efflorescence additive, and 50-100 parts of closed-cell vitrified microspheres.
2. The coating for renovating exposed brick walls according to claim 1, characterized in that: The imitation brick coating also includes: a color repairing layer coated on the surface of the imitation brick decorative mortar layer.
3. The coating for renovating exposed brick walls according to claim 2, characterized in that: The color-correcting layer is formed by coating a color-correcting agent, and the color-correcting agent includes: a second liquid material and a second powder material, and the ratio of the second liquid material to the second powder material is 1:0.5 to 1:2; wherein: The second liquid material comprises, by mass, 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH regulator, 1-3 parts of thickener, and 20-50 parts of inorganic color paste; The second powder comprises, by mass, 400-600 parts of heavy calcium, 200-300 parts of cement, 50-100 parts of gypsum, 1-3 parts of water reducing agent, and 1-3 parts of anti-efflorescence additive.
4. The coating for renovating exposed brick walls according to claim 1, characterized in that: The filling layer is formed by filling with a filling material, and the filling material includes: a third liquid material and a third powder material, and the ratio of the third liquid material to the third powder material is 1:3 to 1:5; wherein: The third liquid material comprises, by mass, 100-300 parts of water, 1-3 parts of preservative, 1-3 parts of cellulose, 1-3 parts of wetting agent, 1-3 parts of dispersant, 2-4 parts of defoaming agent, 50-100 parts of titanium dioxide, 20-50 parts of fiber, 500-700 parts of acrylic emulsion, 20-40 parts of film-forming aid, 5-10 parts of ethylene glycol, 1-2 parts of pH regulator, 1-3 parts of thickener, and 20-50 parts of inorganic color paste; The third powder comprises, by mass, 200 to 400 parts of cement, 600 to 800 parts of glass beads, 1 to 3 parts of water reducing agent, and 1 to 3 parts of anti-efflorescence additive.
5. The coating for renovating exposed brick walls according to any one of claims 1 to 4, characterized in that: The gypsum is alpha gypsum, and the fiber is aluminum silicate fiber.
6. The coating for renovating exposed brick walls according to any one of claims 1 to 4, characterized in that: Also includes: The base coating and the top coating layer, the base coating is used to be coated on the surface of the plain brick wall, the imitation brick coating is coated on the surface of the base coating, and the top coating layer is coated on the surface of the imitation brick coating.
7. The coating for renovating exposed brick walls according to claim 6, characterized in that: The base coat is formed by coating a reinforcing base coat, and the reinforcing base coat comprises, by mass, 100 to 200 parts of acrylic emulsion, 400 to 700 parts of water, 200 to 300 parts of inorganic potassium silicate, and 10 to 20 parts of a film-forming aid.
8. The coating for renovating exposed brick walls according to claim 7, characterized in that: The film-forming aid of the reinforcement primer is ethylene glycol monobutyl ether.
9. The coating for renovating exposed brick walls according to claim 6, characterized in that: The topcoat layer is formed by coating with an isooctylsilane impregnating agent.
10. The construction process for renovating a coating on a plain brick wall according to any one of claims 1 to 9, characterized in that: The imitation brick decorative mortar layer is constructed by batch coating in several steps, and the process is as follows: The first coat of imitation brick decorative mortar is used to level the joints of the exposed brick wall. The cracked and damaged joints need to be cleaned and then leveled; The second coat of imitation brick decorative mortar is used to thicken the imitation brick decorative mortar layer, and the masking paper is pre-embedded to outline the corresponding joints of the plain bricks. After the coating construction is completed, the masking paper is torn off to form joints on the imitation brick decorative mortar layer; The third coat of imitation brick decorative mortar is to shape the surface of the imitation brick decorative mortar layer to achieve the effect of imitating the surface appearance of plain bricks.