Lining thin-wall stainless steel pipe steel wire framework PE composite pipe and production process thereof
By wrapping mesh steel wire outside the steel pipe and using high-temperature resistant epoxy/organosilicon adhesive to form a thin-walled stainless steel pipe wire skeleton PE composite pipe, the problems of poor adhesiveness of composite pipes and easy corrosion of steel pipes are solved, and the problem of poor adhesiveness of composite pipes is achieved. It has corrosion resistance, high temperature resistance and high strength effects.
Patent Information
- Application Number
- CN202411160330.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing composite pipes have poor adhesiveness between steel pipes and plastic pipes, which are easy to detach, and the steel pipes are easily corrosive and costly, and the PE pipes are low in strength.
The production process of PE composite pipe with thin-walled stainless steel pipe wire skeleton PE composite pipe is adopted. By wrapping mesh steel wire outside the steel pipe and using high-temperature epoxy/organosilicon adhesive, a multi-layer structure composite pipe is formed to ensure firm adhesive and resistant corrosion.
The composite pipe is corrosion-resistant, high temperature resistance, water resistance and flame retardancy are achieved, while the strength is improved, the problem of poor adhesiveness is avoided, and a product with good comprehensive performance is formed.
Smart Images

Figure BDA0005006237950000121 
Figure BDA0005006237950000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite pipes, and in particular to a PE composite pipe lined with a thin-wall stainless steel pipe and a steel wire skeleton and a production process thereof. Background Art
[0002] In industrial and agricultural production and urban infrastructure construction, the transportation of pressure media requires extremely high-strength pipes, such as plastic pipes or steel pipes. The former has anti-corrosion and heat-insulating properties, but because it is made of plastic, its strength is relatively low; although the latter has higher strength, it is made of steel and is easily corroded, and the cost is relatively high. In order to enhance the strength and performance of the composite pipe, a plastic pipe can also be used to cover the steel pipe to form a composite pipe, but this composite pipe often has problems such as poor adhesion between the steel pipe and the plastic pipe and easy separation. Summary of the invention
[0003] The purpose of the present invention is to propose a PE composite pipe lined with a thin-wall stainless steel pipe and a steel wire skeleton and a production process thereof. The pipe has low cost, a wide source of raw materials, a simple preparation method, and has good effects of improving immunity, increasing the protein content and immune protein content of goat milk, and is widely used in products for increasing the milk production of dairy goats, improving the quality of goat milk, and reducing ammonia poisoning in dairy goats.
[0004] The technical solution of the present invention is achieved in this way:
[0005] The present invention provides a production process of a PE composite pipe lined with a thin-wall stainless steel pipe and a steel wire skeleton, comprising the following steps:
[0006] (1) The steel strip is passed through a pipe forming machine to form a steel pipe;
[0007] (2) A first steel wire coated with a first adhesive is wound around the outside of the steel pipe, and the first adhesive is melted through a heating process, so that the first steel wire is wound and adhered to the outside of the steel pipe, and the first steel wire is a mesh-shaped cross steel wire;
[0008] (3) winding a second steel wire around the outside of the steel tube around which the first steel wire is wound at an angle to the first steel wire, wherein the second steel wire is a mesh-shaped cross-shaped steel wire, wherein the cross-shaped structure of the second steel wire may be the same as or different from the cross-shaped structure of the first steel wire;
[0009] (4) placing the steel pipe wrapped with two layers of steel wires in a heated and glued state so that the outer surface of the second steel wire is coated with the second adhesive;
[0010] (5) When the second adhesive is not cured, the outer surface of the second steel wire of the steel pipe is wrapped with a PE film to form a steel pipe lining-two layers of steel wire in the middle-external PE lined thin-walled stainless steel pipe steel wire skeleton PE composite pipe;
[0011] The first adhesive and the second adhesive are the same or different.
[0012] As a further improvement of the present invention, the first adhesive is the same as the second adhesive, which is a high temperature resistant epoxy / organic silicone adhesive, and the preparation method is as follows:
[0013] S1. Modification of silicone resin: adding silane coupling agent KH560 to polysiloxane silicone resin, heating and stirring to mix evenly to obtain modified silicone resin;
[0014] S2. Modification of nano-silicon oxide: adding nano-silicon oxide to ethanol, adding a silane coupling agent, heating and stirring the reaction, centrifuging, washing, and drying to obtain modified nano-silicon oxide;
[0015] S3. Chemical vapor deposition: The modified nano-silicon oxide is evenly spread out in the center of a quartz porcelain boat, placed in a tube furnace, heated under inert gas protection, n-hexane is introduced, the reaction is kept warm, and cooled to room temperature under inert gas protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0016] S4. Preparation of flame retardant accelerator: adding hexachlorocyclotriphosphazene and benzyl alcohol to an organic solvent, adding triethylamine dropwise, stirring the reaction at room temperature, adding water to precipitate, filtering, washing, and drying to obtain a flame retardant accelerator;
[0017] S5. Preparation of high temperature resistant epoxy / silicone adhesive: Mix modified silicone resin, epoxy resin and diluent evenly to obtain component A, mix carbon nanotubes / modified nano-silicon oxide, curing agent and flame retardant promoter evenly to obtain component B, and mix component A and component B evenly when using to obtain high temperature resistant epoxy / silicone adhesive.
[0018] As a further improvement of the present invention, the mass ratio of the polysiloxane silicone resin to the silane coupling agent KH560 in step S1 is 100:7-10, the heating and stirring temperature is 45-55° C., and the time is 1-2 h.
[0019] As a further improvement of the present invention, the mass ratio of the nano-silicon oxide to the silane coupling agent in step S2 is 10:1-2, the silane coupling agent is selected from at least one of KH550, KH602, and KH792, and the heating and stirring reaction is performed at a temperature of 40-50° C. for 2-4 hours.
[0020] As a further improvement of the present invention, the temperature in step S3 is raised to 650-670° C., the ventilation rate of n-hexane is 1-2 mL / min, and the insulation reaction time is 20-40 min.
[0021] As a further improvement of the present invention, the molar ratio of hexachlorocyclotriphosphazene, benzyl alcohol and triethylamine in step S4 is 1:6-6.2:10-15, and the reaction time of stirring at room temperature is 3-5 hours.
[0022] As a further improvement of the present invention, the epoxy resin in step S5 is epoxy resin E51 or E44, the mass ratio of the modified silicone resin, epoxy resin and diluent is 10:17-22:1-2; the diluent is diglycidyl ether; the curing agent is meta-phenylenediamine or diaminodiphenylmethane; the mass ratio of the carbon nanotubes / modified nano-silica, curing agent and flame retardant promoter is 1-2:1.5-2.5:1.2-1.5.
[0023] As a further improvement of the present invention, the first adhesive is different from the second adhesive, and the first adhesive or the second adhesive is a high temperature resistant epoxy / silicone adhesive, and the other is an epoxy resin adhesive E51.
[0024] As a further improvement of the present invention, the thickness of the steel pipe is 0.5-1.5 mm, the thickness of the first steel wire layer and the second steel wire layer is 0.1-1.0 mm, the thickness of the PE film is 1-2 mm, and the heating temperature is 150-160°C.
[0025] The present invention further protects a PE composite pipe lined with a thin-wall stainless steel pipe and a steel wire skeleton produced by the above production process.
[0026] The present invention has the following beneficial effects:
[0027] The PE composite pipe with an inner lining of thin-walled stainless steel pipe and a steel wire skeleton prepared by the present invention not only effectively overcomes the problems of low strength of a single PE pipe and corrosion of a single steel pipe and high cost, or the use of an internal or external steel mesh or steel pipe to improve the strength of the PE pipe, but there are problems such as poor adhesion between the steel pipe and the plastic pipe formed in the composite pipe and easy separation. The composite pipe prepared by the present invention is corrosion-resistant, high-temperature resistant, water-resistant, has a certain degree of flame retardancy, and has high strength. At the same time, the adhesive between the multi-layer structure is firmly bonded, not easy to separate, has high peeling strength, and the formed composite pipe has good comprehensive performance.
[0028] The present invention prepares a high temperature resistant epoxy / organic silicone adhesive, and the polysiloxane silicone resin is modified by the silane coupling agent KH560, and the silane coupling agent KH560 can significantly improve the high temperature resistance. The silane coupling agent KH560 acts as a transition phase and plays a bridging role at the interface between the epoxy resin and the silicone resin, significantly improving the compatibility of the epoxy resin and the silicone resin, reducing the internal stress of the system, and thus improving the high temperature resistance.
[0029] After the surface of nano silicon oxide is modified by silane coupling agent, carbon nanotubes are deposited on the surface. On the one hand, the modified silane coupling agent side chain can be easily entangled with the molecular weight of epoxy resin, improving the dispersibility of nanoparticles. At the same time, after the carbon nanotubes are deposited, the surface forms a wrinkled shape, reducing the agglomeration in the resin matrix, achieving uniform dispersion, and greatly improving its toughness and strength. At the same time, since the particles are evenly dispersed in the resin matrix, when the matrix is impacted, the silver streaks generated between the particles and the matrix can absorb a large amount of impact energy and prevent the spread of the silver streaks: at the same time, the matrix between the particles also produces plastic deformation, absorbing the impact energy, thereby achieving the effect of toughening. In addition, the amino structure of the nanoparticles modified by the silane coupling agent with amino groups can also react with epoxy groups to play a part of the curing agent.
[0030] The flame retardant accelerator prepared by the invention takes hexachlorocyclotriphosphazene as a main component and reacts with benzyl alcohol to form an organic phosphine structure flame retardant accelerator, which has the characteristics of NP flame retardant and has good compatibility with resin system, high catalytic activity, storage stability, low hygroscopicity, excellent heat resistance, high decomposition temperature, and can be synergistically cured with amine curing agent, thereby greatly reducing the amount of curing agent.
[0031] In addition, the epoxy resin and silicone resin matrix of the present invention are the main materials, and the nanoparticles are used for toughening. After curing, the epoxy resin and silicone resin matrix have good mechanical strength and corrosion resistance, and the high temperature resistance and flame retardancy are also significantly improved. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Polysiloxane silicone resin SAR-9, light yellow uniform liquid, solid content 51%, viscosity 30-35MPa·s.
[0034] The particle size range of nano silicon oxide is 150±50nm.
[0035] Preparation Example 1 Preparation of high temperature resistant epoxy / organic silicone adhesive
[0036] The specific steps include:
[0037] S1. Modification of silicone resin: 7 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 45 ° C, stirred and reacted for 1 h to obtain a modified silicone resin;
[0038] S2. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 1 g of silane coupling agent KH550 was added, heated to 40 ° C, stirred for 2 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0039] S3. Chemical vapor deposition: 10 g of modified nano-silicon oxide was evenly spread in the center of a quartz boat, placed in a tube furnace, heated to 650 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 1 mL / min. The reaction was kept warm for 20 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0040] S4. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.6 mol benzyl alcohol were added to 200 mL acetonitrile, 1 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 3 h, an equal volume of water was added to precipitate, filtered, washed, and dried to obtain a flame retardant accelerator;
[0041] S5. Preparation of high temperature resistant epoxy / silicone adhesive: stir and mix 10g of modified silicone resin, 17g of epoxy resin E51 and 1g of diglycidyl ether for 15 minutes to obtain component A, stir and mix 1g of carbon nanotubes / modified nano-silica, 1.5g of meta-phenylenediamine and 1.2g of flame retardant promoter for 15 minutes to obtain component B. When using, stir and mix components A and B for 15 minutes and cure for 1 hour to obtain a high temperature resistant epoxy / silicone adhesive.
[0042] Preparation Example 2 Preparation of high temperature resistant epoxy / organic silicone adhesive
[0043] The specific steps include:
[0044] S1. Modification of silicone resin: 10 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 55 ° C, stirred and reacted for 2 h to obtain a modified silicone resin;
[0045] S2. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 2 g of silane coupling agent KH602 was added, heated to 50°C, stirred for 4 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0046] S3. Chemical vapor deposition: 10 g of modified nano-silicon oxide was evenly spread in the center of a quartz porcelain boat, placed in a tube furnace, heated to 670 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 2 mL / min. The reaction was kept warm for 40 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0047] S4. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.62 mol benzyl alcohol were added to 200 mL acetonitrile, 1.5 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 5 h, an equal volume of water was added to precipitate, filtered, washed, and dried to obtain a flame retardant accelerator;
[0048] S5. Preparation of high temperature resistant epoxy / silicone adhesive: 10 g of modified silicone resin, 22 g of epoxy resin E51 and 2 g of diglycidyl ether were stirred and mixed for 15 min to obtain component A; 2 g of carbon nanotubes / modified nano-silica, 2.5 g of diaminodiphenylmethane and 1.5 g of flame retardant promoter were stirred and mixed for 15 min to obtain component B. When using, component A and component B were stirred and mixed for 15 min, and cured for 1 h to obtain a high temperature resistant epoxy / silicone adhesive.
[0049] Preparation Example 3 Preparation of high temperature resistant epoxy / organic silicone adhesive
[0050] The specific steps include:
[0051] S1. Modification of silicone resin: 8.5 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 50 ° C, stirred and reacted for 1.5 h to obtain a modified silicone resin;
[0052] S2. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 1.5 g of silane coupling agent KH792 was added, heated to 45 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0053] S3. Chemical vapor deposition: 10 g of modified nano-silicon oxide was evenly spread in the center of a quartz boat, placed in a tube furnace, heated to 660 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 1.5 mL / min. The reaction was kept warm for 30 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0054] S4. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.61 mol benzyl alcohol were added to 200 mL acetonitrile, 1.2 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 4 h, an equal volume of water was added to precipitate, filtered, washed, and dried to obtain a flame retardant accelerator;
[0055] S5. Preparation of high temperature resistant epoxy / silicone adhesive: 10 g of modified silicone resin, 20 g of epoxy resin E51 and 1.2 g of diglycidyl ether were stirred and mixed for 15 minutes to obtain component A, 1.5 g of carbon nanotubes / modified nano-silica, 2 g of meta-phenylenediamine and 1.35 g of flame retardant promoter were stirred and mixed for 15 minutes to obtain component B. When using, component A and component B were stirred and mixed for 15 minutes and cured for 1 hour to obtain high temperature resistant epoxy / silicone adhesive.
[0056] Comparative Preparation Example 1
[0057] Compared with Preparation Example 3, the difference is that step S1 is not performed.
[0058] The details are as follows:
[0059] S1. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 1.5 g of silane coupling agent KH792 was added, heated to 45°C, stirred for reaction for 3 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0060] S2. Chemical vapor deposition: 10 g of modified nano-silicon oxide was evenly spread in the center of a quartz boat, placed in a tube furnace, heated to 660 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 1.5 mL / min. The reaction was kept warm for 30 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0061] S3. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.61 mol benzyl alcohol were added to 200 mL acetonitrile, 1.2 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 4 h, an equal volume of water was added to precipitate, filtered, washed and dried to obtain a flame retardant accelerator;
[0062] S4. Preparation of high temperature resistant epoxy / silicone adhesive: stir and mix 10g of polysiloxane silicone resin SAR-9, 20g of epoxy resin E51 and 1.2g of diglycidyl ether for 15 minutes to obtain component A, stir and mix 1.5g of carbon nanotubes / modified nano-silica, 2g of meta-phenylenediamine and 1.35g of flame retardant accelerator for 15 minutes to obtain component B. When using, stir and mix components A and B for 15 minutes, and cure for 1 hour to obtain a high temperature resistant epoxy / silicone adhesive.
[0063] Comparative Preparation Example 2
[0064] Compared with Preparation Example 3, the difference is that step S2 is not performed.
[0065] The details are as follows:
[0066] S1. Modification of silicone resin: 8.5 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 50 ° C, stirred and reacted for 1.5 h to obtain a modified silicone resin;
[0067] S2. Chemical vapor deposition: 10 g of nano-silicon oxide was evenly spread in the center of a quartz porcelain boat, placed in a tube furnace, heated to 660 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 1.5 mL / min. The reaction was kept warm for 30 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / nano-silicon oxide;
[0068] S3. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.61 mol benzyl alcohol were added to 200 mL acetonitrile, 1.2 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 4 h, an equal volume of water was added to precipitate, filtered, washed and dried to obtain a flame retardant accelerator;
[0069] S4. Preparation of high temperature resistant epoxy / silicone adhesive: stir and mix 10g of modified silicone resin, 20g of epoxy resin E51 and 1.2g of diglycidyl ether for 15 minutes to obtain component A, stir and mix 1.5g of carbon nanotubes / nanosilica, 2g of meta-phenylenediamine and 1.35g of flame retardant promoter for 15 minutes to obtain component B. When using, stir and mix components A and B for 15 minutes, and cure for 1 hour to obtain a high temperature resistant epoxy / silicone adhesive.
[0070] Comparative Preparation Example 3
[0071] Compared with Preparation Example 3, the difference is that step S3 is not performed.
[0072] The details are as follows:
[0073] S1. Modification of silicone resin: 8.5 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 50 ° C, stirred and reacted for 1.5 h to obtain a modified silicone resin;
[0074] S2. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 1.5 g of silane coupling agent KH792 was added, heated to 45 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0075] S3. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.61 mol benzyl alcohol were added to 200 mL acetonitrile, 1.2 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 4 h, an equal volume of water was added to precipitate, filtered, washed and dried to obtain a flame retardant accelerator;
[0076] S4. Preparation of high temperature resistant epoxy / silicone adhesive: 10g of modified silicone resin, 20g of epoxy resin E51 and 1.2g of diglycidyl ether were stirred and mixed for 15 minutes to obtain component A, 1.5g of modified nano-silica, 2g of meta-phenylenediamine and 1.35g of flame retardant promoter were stirred and mixed for 15 minutes to obtain component B. When using, component A and component B were stirred and mixed for 15 minutes and cured for 1 hour to obtain high temperature resistant epoxy / silicone adhesive.
[0077] Comparative Preparation Example 4
[0078] Compared with Preparation Example 3, the difference is that the flame retardant promoter is replaced by triphenylphosphine.
[0079] The details are as follows:
[0080] S1. Modification of silicone resin: 8.5 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 50 ° C, stirred and reacted for 1.5 h to obtain a modified silicone resin;
[0081] S2. Modification of nano-silicon oxide: 10 g of nano-silicon oxide was added to 200 mL of ethanol, 1.5 g of silane coupling agent KH792 was added, heated to 45 ° C, stirred for 3 h, centrifuged, washed, and dried to obtain modified nano-silicon oxide;
[0082] S3. Chemical vapor deposition: 10 g of modified nano-silicon oxide was evenly spread in the center of a quartz boat, placed in a tube furnace, heated to 660 ° C under nitrogen protection, and n-hexane was introduced at a flow rate of 1.5 mL / min. The reaction was kept warm for 30 min and cooled to room temperature under nitrogen protection to obtain carbon nanotubes / modified nano-silicon oxide;
[0083] S4. Preparation of high temperature resistant epoxy / silicone adhesive: 10 g of modified silicone resin, 20 g of epoxy resin E51 and 1.2 g of diglycidyl ether were stirred and mixed for 15 minutes to obtain component A, 1.5 g of carbon nanotubes / modified nano-silica, 2 g of meta-phenylenediamine and 1.35 g of triphenylphosphine were stirred and mixed for 15 minutes to obtain component B. When using, component A and component B were stirred and mixed for 15 minutes and cured for 1 hour to obtain a high temperature resistant epoxy / silicone adhesive.
[0084] Comparative Preparation Example 5
[0085] Compared with Preparation Example 3, the difference is that no carbon nanotubes / modified nano-silicon oxide is added.
[0086] The details are as follows:
[0087] S1. Modification of silicone resin: 8.5 g of silane coupling agent KH560 was added to 100 g of polysiloxane silicone resin SAR-9, heated to 50 ° C, stirred and reacted for 1.5 h to obtain a modified silicone resin;
[0088] S2. Preparation of flame retardant accelerator: 0.1 mol hexachlorocyclotriphosphazene and 0.61 mol benzyl alcohol were added to 200 mL acetonitrile, 1.2 mol triethylamine was added dropwise, the reaction was stirred at room temperature for 4 h, an equal volume of water was added to precipitate, filtered, washed, and dried to obtain a flame retardant accelerator;
[0089] S3. Preparation of high temperature resistant epoxy / silicone adhesive: stir and mix 10g of modified silicone resin, 20g of epoxy resin E51 and 1.2g of diglycidyl ether for 15 minutes to obtain component A, stir and mix 3.5g of meta-phenylenediamine and 1.35g of flame retardant promoter for 15 minutes to obtain component B. When using, stir and mix components A and B for 15 minutes and cure for 1 hour to obtain a high temperature resistant epoxy / silicone adhesive.
[0090] Test Example 1
[0091] The performance of the high temperature resistant epoxy / silicone adhesives prepared in Preparation Examples 1-3 and Comparative Examples 1-5 was tested.
[0092] Room temperature shear strength is in accordance with GB / T 7124-2008, high temperature shear strength is in accordance with GJB / 444-1988, the test piece material is LY12CZ aluminum alloy, specification is 60mm×20mm×3mm, bonding area is: 20mm×15mm.
[0093] The limiting oxygen index (LOI) is tested according to GB / T2406.2-2009 standard by making the sample into a shape of 100mm×10mm×4mm.
[0094] The results are shown in Table 1.
[0095] Table 1
[0096]
[0097] It can be seen from the above table that the high temperature resistant epoxy / silicone adhesives prepared in Preparation Examples 1-3 of the present invention have good mechanical properties, high temperature resistance and flame retardant properties.
[0098] Example 1
[0099] This embodiment provides a production process for a PE composite pipe lined with a thin-walled stainless steel pipe and a steel wire skeleton, comprising the following steps:
[0100] S1. The steel strip is formed into a steel pipe through a pipe forming machine with a thickness of 1 mm;
[0101] S2. A first steel wire having a first adhesive coated on its surface is wound around the outside of the steel pipe, and the first adhesive is melted by heating to 150° C., so that the first steel wire is wound and adhered to the outside of the steel pipe, and the first steel wire is a mesh-shaped cross steel wire;
[0102] S3. Wrapping the second steel wire around the outside of the steel tube around which the first steel wire is wrapped at an angle to the first steel wire, wherein the second steel wire is a mesh-shaped cross-shaped steel wire, wherein the cross-shaped structure of the second steel wire may be the same as or different from the cross-shaped structure of the first steel wire;
[0103] S4. The steel pipe wrapped with two layers of steel wire is heated to 150°C, and the outer surface of the second steel wire is coated with a second adhesive in the glue-coated state;
[0104] S5. When the second adhesive is not cured, the outer surface of the second steel wire of the steel pipe is wrapped with a PE film to form a steel pipe liner - two layers of steel wire in the middle - an outer PE lined thin-walled stainless steel pipe steel wire skeleton PE composite pipe;
[0105] The thickness of the first steel wire layer and the second steel wire layer is 0.5 mm; the thickness of the PE film is 2 mm;
[0106] Among them, the first adhesive and the second adhesive are the same, which is the high temperature resistant epoxy / organic silicone adhesive prepared in Preparation Example 1.
[0107] Example 2
[0108] This embodiment provides a production process for a PE composite pipe lined with a thin-walled stainless steel pipe and a steel wire skeleton, comprising the following steps:
[0109] S1. The steel strip is formed into a steel pipe through a pipe forming machine with a thickness of 1 mm;
[0110] S2. A first steel wire having a first adhesive coated on its surface is wound around the outside of the steel pipe, and the first adhesive is melted by heating to 160° C., so that the first steel wire is wound and adhered to the outside of the steel pipe, and the first steel wire is a mesh-shaped cross steel wire;
[0111] S3. Wrapping the second steel wire around the outside of the steel tube around which the first steel wire is wrapped at an angle to the first steel wire, wherein the second steel wire is a mesh-shaped cross-shaped steel wire, wherein the cross-shaped structure of the second steel wire may be the same as or different from the cross-shaped structure of the first steel wire;
[0112] S4. The steel pipe wrapped with two layers of steel wire is heated to 160°C, so that the outer surface of the second steel wire is coated with a second adhesive;
[0113] S5. When the second adhesive is not cured, the outer surface of the second steel wire of the steel pipe is wrapped with a PE film to form a steel pipe liner - two layers of steel wire in the middle - an outer PE lined thin-walled stainless steel pipe steel wire skeleton PE composite pipe;
[0114] The thickness of the first steel wire layer and the second steel wire layer is 0.5 mm; the thickness of the PE film is 2 mm;
[0115] Among them, the first adhesive is the high temperature resistant epoxy / silicone adhesive prepared in Preparation Example 2, and the second adhesive is epoxy resin E51.
[0116] Example 3
[0117] This embodiment provides a production process for a PE composite pipe lined with a thin-walled stainless steel pipe and a steel wire skeleton, comprising the following steps:
[0118] S1. The steel strip is formed into a steel pipe through a pipe forming machine with a thickness of 1 mm;
[0119] S2. A first steel wire having a first adhesive coated on its surface is wound around the outside of the steel pipe, and the first adhesive is melted by heating to 155° C., so that the first steel wire is wound and adhered to the outside of the steel pipe, and the first steel wire is a mesh-shaped cross steel wire;
[0120] S3. Wrapping the second steel wire around the outside of the steel tube around which the first steel wire is wrapped at an angle to the first steel wire, wherein the second steel wire is a mesh-shaped cross-shaped steel wire, wherein the cross-shaped structure of the second steel wire may be the same as or different from the cross-shaped structure of the first steel wire;
[0121] S4. The steel pipe wrapped with two layers of steel wire is heated to 155°C, so that the outer surface of the second steel wire is coated with a second adhesive;
[0122] S5. When the second adhesive is not cured, the outer surface of the second steel wire of the steel pipe is wrapped with a PE film to form a steel pipe liner - two layers of steel wire in the middle - an outer PE lined thin-walled stainless steel pipe steel wire skeleton PE composite pipe;
[0123] The thickness of the first steel wire layer and the second steel wire layer is 0.5 mm; the thickness of the PE film is 2 mm;
[0124] Among them, the first adhesive and the second adhesive are the high temperature resistant epoxy / silicone adhesive prepared in Preparation Example 3.
[0125] Comparative Examples 1-5
[0126] Compared with Example 3, the difference is that the high temperature resistant epoxy / silicone adhesive is prepared by Comparative Preparation Examples 1-5 respectively.
[0127] Comparative Example 6
[0128] Compared with Example 3, the difference is that the second steel wire layer is not provided.
[0129] Comparative Example 7
[0130] Compared with Example 3, the difference is that the first steel wire layer and the second steel wire layer are not provided, and the steel tube layer and the PE layer are bonded with a high temperature resistant epoxy / organic silicone adhesive.
[0131] Test Example 1
[0132] After curing the thin-walled stainless steel tube lined steel wire skeleton PE composite pipes prepared in Examples 1-3 and Comparative Examples 1-7 for 72 hours at room temperature, the tensile strength and shear strength at 25°C and 150°C were measured respectively according to the GB / T 228-2010 method. The results are shown in Table 2.
[0133] Table 2
[0134]
[0135] It can be seen from the above table that the thin-walled stainless steel tube lined steel wire skeleton PE composite pipes prepared in Examples 1-3 of the present invention have greater strength and better high temperature resistance.
[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A production process for a thin-walled stainless steel lined steel wire skeleton PE composite pipe. It is characterized in that The following steps are involved: (1) The steel strip is passed through a pipe forming machine to form a steel pipe; (2) A first steel wire coated with a first adhesive is wound around the outside of the steel pipe, and the first adhesive is melted through a heating process, so that the first steel wire is wound and adhered to the outside of the steel pipe, and the first steel wire is a mesh-shaped cross steel wire; (3) winding a second steel wire around the outside of the steel tube around which the first steel wire is wound at an angle to the first steel wire, wherein the second steel wire is a mesh-shaped cross-shaped steel wire, wherein the cross-shaped structure of the second steel wire is the same as or different from the cross-shaped structure of the first steel wire; (4) placing the steel pipe wrapped with two layers of steel wires in a heated and glued state so that the outer surface of the second steel wire is coated with the second adhesive; (5) When the second adhesive is not cured, the outer surface of the second steel wire of the steel pipe is wrapped with a PE film to form a steel pipe lining-two layers of steel wire in the middle-external PE lined thin-walled stainless steel pipe steel wire skeleton PE composite pipe; The first adhesive and the second adhesive are the same or different.
2. The production process according to claim 1, It is characterized in that The first adhesive is the same as the second adhesive, which is a high temperature resistant epoxy / organic silicone adhesive, and the preparation method is as follows: S1. Modification of silicone resin: adding silane coupling agent KH560 to polysiloxane silicone resin, heating and stirring to mix evenly to obtain modified silicone resin; S2. Modification of nano-silicon oxide: adding nano-silicon oxide to ethanol, adding a silane coupling agent, heating and stirring the reaction, centrifuging, washing, and drying to obtain modified nano-silicon oxide; S3. Chemical vapor deposition: The modified nano-silicon oxide is evenly spread out in the center of a quartz porcelain boat, placed in a tube furnace, heated under inert gas protection, n-hexane is introduced, the reaction is kept warm, and cooled to room temperature under inert gas protection to obtain carbon nanotubes / modified nano-silicon oxide; S4. Preparation of flame retardant accelerator: adding hexachlorocyclotriphosphazene and benzyl alcohol to an organic solvent, adding triethylamine dropwise, stirring the reaction at room temperature, adding water to precipitate, filtering, washing, and drying to obtain a flame retardant accelerator; S5. Preparation of high temperature resistant epoxy / silicone adhesive: Mix modified silicone resin, epoxy resin and diluent evenly to obtain component A, mix carbon nanotubes / modified nano-silicon oxide, curing agent and flame retardant promoter evenly to obtain component B, and mix component A and component B evenly when using to obtain high temperature resistant epoxy / silicone adhesive.
3. The production process according to claim 2, It is characterized in that In step S1, the mass ratio of the polysiloxane silicone resin to the silane coupling agent KH560 is 100:7-10, the heating and stirring temperature is 45-55° C., and the time is 1-2 h.
4. The production process according to claim 2, It is characterized in that In step S2, the mass ratio of nano silicon oxide to silane coupling agent is 10:1-2, the silane coupling agent is selected from at least one of KH550, KH602, and KH792, and the temperature of the heating and stirring reaction is 40-50° C. and the time is 2-4 hours.
5. The production process according to claim 2, It is characterized in that In step S3, the temperature is raised to 650-670° C., the ventilation rate of n-hexane is 1-2 mL / min, and the insulation reaction time is 20-40 min.
6. The production process according to claim 2, It is characterized in that In step S4, the molar ratio of hexachlorocyclotriphosphazene, benzyl alcohol and triethylamine is 1:6-6.2:10-15, and the reaction time under room temperature stirring is 3-5 hours.
7. The production process according to claim 2, It is characterized in that The epoxy resin in step S5 is epoxy resin E51 or E44, the mass ratio of the modified silicone resin, epoxy resin and diluent is 10:17-22:1-2; the diluent is diglycidyl ether; the curing agent is m-phenylenediamine or diaminodiphenylmethane; the mass ratio of the carbon nanotubes / modified nano-silica, curing agent and flame retardant accelerator is 1-2:1.5-2.5:1.2-1.
5.
8. The production process according to claim 2, It is characterized in that The first adhesive is different from the second adhesive. The first adhesive or the second adhesive is a high temperature resistant epoxy / silicone adhesive, and the other is an epoxy resin adhesive E51.
9. The production process according to claim 1, It is characterized in that The thickness of the steel pipe is 0.5-1.5 mm, the thickness of the first steel wire layer and the second steel wire layer is 0.1-1.0 mm, the thickness of the PE film is 1-2 mm, and the heating temperature is 150-160°C.
10. A PE composite pipe lined with a thin-walled stainless steel pipe and a steel wire skeleton produced by the production process according to any one of claims 1 to 9.
Citation Information
Patent Citations
Metal mesh plastic composite pipe winded with reinforced structure and preparation method thereof
CN101158424A
Composite pipe concrete composite structure
CN102936941A
Production process of steel wire mesh framework polyethylene composite pipe and composite pipe prepared by production process
CN112477213A
Adhesive composition
JP1999323297A
Composite Pipe
KR102419264B1