Chloride ion detection method and device based on porous anion exchange resin / perovskite nanocrystalline multilayer probe

The RGB value is detected by porous anion exchange resin/perovskite nanocrystal multi-layer probe combined with color sensor to establish a chloride ion concentration model, solving the cost and complexity of the existing chloride ion detection methods, and achieving rapid chloride ion concentration Convenient and real-time detection to meet portable and cost-effective needs.

CN119044078APending Publication Date: 2024-11-29JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411167451.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing chloride ion detection methods require expensive instruments, complex operations and cumbersome wastewater pretreatment, which cannot be conducted on-site real-time inspection, and have strict requirements on water quality, which cannot meet portable and cost-effective needs.

Method used

Using porous anion exchange resin/perovskite nanocrystal multilayer probe, the combination of perovskite CsPbBr3 nanocrystals and anionic resin is prepared, and the halide exchange performance with chloride ions is used to detect RGB values ​​in combination with color sensors to establish chloride ions. Concentration model to achieve convenient chloride ion detection.

Benefits of technology

It realizes fast, convenient and real-time detection of chloride ion concentration, reduces detection costs, improves detection accuracy and efficiency, and has low pollution and non-toxicity, making it suitable for rapid detection of chloride ion in various scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044078A_ABST
    Figure CN119044078A_ABST
Patent Text Reader

Abstract

The invention discloses a chloride ion detection method and device based on a porous anion exchange resin / perovskite nanocrystalline multilayer probe. The chloride ion concentration of a solution to be detected is rapidly detected through an exchange channel established by anion exchange resin and the affinity of perovskite nanocrystalline added with metal elements to chloride ions. The detection method comprises the following steps: immersing the detection pen into a to-be-detected solution; the porous anion exchange resin / perovskite nanocrystalline multi-layer probe CsPbBr3 (at) Resin (CPB (at) Resin) subjected to ion exchange shows color change; the obtained RGB value is transmitted back to the master controller to be processed, the detection device is used for calculating to obtain chloride ion concentration data, and the cost benefit of detecting chloride ions in water is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a chloride ion detection method and device based on a porous anion exchange resin / perovskite nanocrystal multilayer probe. Background Art

[0002] Chloride ions are widely present in water bodies, usually in the form of chloride salts such as sodium chloride, calcium chloride, potassium chloride, and magnesium chloride. However, high concentrations of chloride ions can cause dehydration and death of plants and microorganisms. In addition, high concentrations of chloride ions can corrode metal pipes, causing toxic metal substances to be released from the pipes. Therefore, it is necessary to monitor the concentration level of chloride ions in water. At present, commonly used chloride ion detection methods include titration, spectrophotometry, ion chromatography, and electrochemical methods. Although these methods have high accuracy and precision, they usually require expensive instruments, complex operations, cumbersome wastewater pretreatment processes, and have strict requirements on water quality, and cannot be detected on site in real time. In recent years, emerging detection technologies have continued to emerge, among which spectrochemical sensors based on nanomaterials have been favored by many researchers for their low price, high selectivity, simple operation, and high efficiency.

[0003] Cesium lead bromide perovskite nanocrystals (CsPbBr3 NCs) have excellent halide exchange properties with chlorine (Cl) and are therefore suitable for the treatment of Cl - The rapid response of CsPbBr3 NCs makes them very suitable for Cl - Detection sensor. Therefore, it is necessary to develop a simple, portable and cost-effective chloride ion detection method and device. Summary of the invention

[0004] The present invention aims to solve the problems existing in the above-mentioned prior art and provides a method and device for detecting chloride ions based on a porous anion exchange resin / perovskite nanocrystal multilayer probe.

[0005] The technical solutions adopted in the present invention are:

[0006] A method for detecting chloride ions based on a porous anion exchange resin / perovskite nanocrystal multilayer probe comprises the following steps:

[0007] S1. Preparation of porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin;

[0008] S2. exchanging the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin prepared in S1 with a chloride ion solution to obtain the reacted CPB@Resin and using a color sensor to detect the reacted CPB@Resin to obtain RGB parameters of multiple sets of three-channel images;

[0009] S3. Use Origin fitting data to establish RGB and C parameters on R, G, B. Cl- Concentration model: C Cl- =kB(RG)+b, where C Cl- is the chloride ion concentration, R, G, B are the values ​​of the red, yellow, and blue color channels respectively, and k and b are coefficients;

[0010] S4. Writing the obtained concentration model into the master controller to form a built-in program;

[0011] S5. Using a chloride ion detection device based on a porous anion exchange resin / perovskite nanocrystal multilayer probe, the chloride ion concentration is calculated through a built-in program and the data is output.

[0012] Furthermore, the preparation process of the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin in S1 includes the following specific steps:

[0013] S11. The perovskite CsPbBr3 nanocrystalline powder is prepared by a hot injection synthesis method, which has good stability in water and is prepared by the following method:

[0014] 1) Add 1-2g Cs2CO3, 3-10mL OA, 10-20mL ODE and 0.01-0.05g metal compound (cuprous bromide, bismuth bromide, silver bromide and antimony bromide) to a 100mL glass three-necked flask, and heat for about 0.5-1.5h under vacuum at 130-180℃ until Cs2CO3 is completely dissolved to generate cesium oleate (Cs-OA) with a small amount of metal remaining. Then, change the vacuum to nitrogen to remove the remaining impurity gas in the system. After 20-50min, 10-30mL 0.3-0.8mmol / mL Cs-OA solution can be obtained. Transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to 100-150℃ to melt it when it is used;

[0015] 2) Weigh 0.1-0.2 g of lead bromide (PbBr2), pipette 10-20 mL of ODE, 0.5-1.5 mL of OA, and 0.5-1.5 mL of OLA, mix and add into a 80-150 mL three-necked flask, and put in a magnetic stirrer. First, evacuate for 20-50 min, then heat in a heating mantle under vacuum at 100-150 ° C for 20-50 min to completely dissolve PbBr2;

[0016] 3) Insert the thermometer into the three-necked flask under nitrogen protection. When the temperature reaches 150-180°C, use a syringe to absorb 0.1-0.3 mL of Cs-OA solution that has been heated and melted in advance, and immediately inject it into the flask. After stirring for 5-10 seconds, quickly transfer the solution out of the flask and cool it in an ice water bath.

[0017] 4) Add 5-15 mL of n-hexane and 10-20 mL of acetone solution to the cooled solution, centrifuge at 10,000-12,000 rpm, and discard the supernatant in the centrifuge tube;

[0018] 5) After centrifuging the above solution, the solid is placed in a vacuum drying oven for further drying to remove the liquid adsorbed on the surface of the solid, thereby obtaining perovskite CsPbBr3 nanocrystalline powder;

[0019] Its photoelectric properties can be tuned by doping with different metal elements, thereby increasing its affinity for chloride ions.

[0020] S12. An anionic resin solution is prepared by an amination scheme, which is prepared by the following method:

[0021] 10-30g chlorine balls (4-7% DVB, chlorine content 500-600mmol / g) are swollen with 150-250mL dimethylformamide, and then 3 times the amount of tertiary amine (tri-n-butylamine, N-ethylguanidine, N,N-dimethylaniline, trimethylamine) is added, and the mixture is left overnight. The next day, the mixture is filtered to obtain an anion resin solution;

[0022] S13. Prepare an anion exchange membrane required for a porous anion exchange resin / perovskite nanocrystal multilayer probe, wherein the preparation method comprises the following operations:

[0023] In the anion exchange resin solution, the content of the anion exchange resin is 5-40wt%, and the anion exchange resin solution is used for scraping to obtain the anion exchange membrane. The scraping temperature is 40-120° C., and the thickness of the anion exchange membrane is 10-50nm;

[0024] S14. Prepare a porous anion exchange resin / perovskite nanocrystal multilayer probe, the specific method is as follows:

[0025] The perovskite CsPbBr3 nanocrystal powder is evenly applied on the anion exchange membrane, and finally the anion exchange membrane is filled again to complete the encapsulation, thereby preparing a porous anion exchange resin / perovskite nanocrystal multilayer probe;

[0026] The porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin can change the pore size of the anion resin by changing the dosage of dimethylformamide and the swelling time during the swelling process to cope with the influence of various other coexisting ions contained in different chloride ion solutions on the detection, and better protect the CsPbBr3 nanocrystals encapsulated by the anion resin in CPB@Resin.

[0027] Furthermore, the detection requires the plotting of a concentration standard curve in advance, and the data of the obtained standard values ​​of different concentrations are fitted to obtain a curve of concentration and R, G, and B values, including: using Origin to fit the data of the obtained standard values ​​of different concentrations to obtain a model of concentration and R, G, and B values.

[0028] Furthermore, the S2 comprises the following specific steps:

[0029] S21. Immerse the union-exchanged CPB@Resin in a solution containing chloride ions and allow to stand for 1 to 5 minutes to obtain the ion-exchanged CPB@Resin;

[0030] S22. Using a UV lamp with a wavelength of 365 nm built into the detection pen to irradiate the CPB@Resin after ion exchange, so as to stimulate it to produce a color that can be better detected by the color sensor;

[0031] S23. Detect the exchanged CPB@Resin through a color sensor to obtain an RGB value.

[0032] Further, in S3, the relationship between the determined RGB value and the chloride ion concentration can be obtained by the following steps:

[0033] S31. Prepare chloride ion solutions of different concentrations to react with CPB@Resin that has not undergone ion exchange;

[0034] S32. Using ultraviolet light with a wavelength of 280 to 380 nm to irradiate the ion-exchanged CPB@Resin, so as to excite the CPB@Resin to produce a color that can be better detected by the color sensor;

[0035] S33. Performing color detection on the CPB@Resin to be tested under the same environment by using a color sensor to obtain RGB values ​​corresponding to the CPB@Resin after ion exchange at different concentrations;

[0036] S34. According to the measured RGB value and the corresponding chloride ion model of the solution / powder, Origin is used to fit the data to obtain a model of RGB value and chloride ion concentration;

[0037] The ion-exchanged CPB@Resin can be immersed in a solution containing bromide ions and allowed to stand for 5 to 10 minutes. After secondary ion exchange, it can be regenerated into new CPB@Resin. The service life of CPB@Resin is not less than 100 ion cycle exchanges.

[0038] The present invention also discloses a detection device, including a host, a mechanical arm and a detection pen. The detection pen is fixed to the mechanical arm, and an ion exchange chamber, an ultraviolet lamp and a color sensor are arranged on the detection pen. A porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin is arranged in the ion exchange chamber. The CPB@Resin is formed by evenly applying perovskite CsPbBr3 nanocrystal powder on an anion exchange membrane. The ultraviolet lamp is used to emit ultraviolet light and irradiate the CPB@Resin. The color sensor is used to detect the RGB value of the light emitted by the CPB@Resin and transmit the RGB value to the host.

[0039] Furthermore, the host is provided with an OLED screen.

[0040] Furthermore, a placement rack is fixed to the end of the mechanical arm, and the detection pen is fixed on the placement rack.

[0041] The present invention has the following beneficial effects:

[0042] 1) The present invention utilizes the property that bromide ions in the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin are easy to exchange ions with external chloride ions, and is used as a fluorescent probe in the chloride ion detection device, and the chloride ion concentration data can be quickly and conveniently obtained.

[0043] 2) The present invention utilizes the protective effect of the anion exchange resin in the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin and the established exchange channels to improve the stability of CsPbBr3 nanocrystals in aqueous solution while better completing ion exchange.

[0044] 3) The present invention utilizes CsPbBr3 nanocrystals doped with metal elements having affinity for chloride ions in the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin, which can not only adjust its photoelectric properties but also enhance the stability and improve the selectivity of the device.

[0045] 4) The present invention utilizes the renewable property of the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin. The adopted technical solution is low in pollution and non-toxic, which improves the detection safety, reduces the detection cost, and improves the detection accuracy and efficiency. The chloride ion concentration is calculated by the built-in program, and the data can be directly obtained from the screen, which is more intuitive and convenient. Real-time online detection has been realized, which can meet the needs of rapid detection of chloride ions in various scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Schematic diagram of the detection device of the present invention.

[0047] Figure 2 Schematic diagram of the detection pen.

[0048] Figure 3 Schematic diagram of the detection method of the present invention.

[0049] Figure 4 Schematic diagram of the structure of the porous anion exchange resin / perovskite nanocrystal multilayer probe.

[0050] Figure 5 This is a graph showing the relationship between the R, G, B values ​​of the captured color and the concentration of added chloride ions.

[0051] Figure 6 A schematic diagram of a computer device according to the present invention.

[0052] 1-host; 2-button; 3-OLED screen; 4-mechanical arm; 5-detection pen; 6-placing rack; 51-pen body; 52-rubber cover; 53-ion exchange chamber; 54-ultraviolet lamp; 55-color sensor. DETAILED DESCRIPTION

[0053] The present invention will be further described below in conjunction with the accompanying drawings.

[0054] Example 1

[0055] like Figure 1 and Figure 2 A chloride ion detection device based on a porous anion exchange resin / perovskite nanocrystal multilayer probe comprises a host 1, a mechanical arm 4 and a detection pen 5. The host 1 is provided with a button 2 and an OLED screen 3, and the button 2, the OLED screen 3 and the detection pen 5 are all electrically connected to a master controller (not shown) in the host 1.

[0056] A placement rack 7 is fixed at the end of the mechanical arm 4 , and the detection pen 5 is fixed on the placement rack 7 .

[0057] The detection pen 5 is provided with an ion exchange chamber 53 , an ultraviolet lamp 54 and a color sensor 55 . The color sensor 55 is used for detecting the object to be detected. The color sensor 55 is installed at the lower end of the pen body 51 .

[0058] A rubber sleeve 52 for holding is sleeved on the middle and lower part of the pen body 51 , a color sensor 55 is fixedly connected to the lower end of the pen body, and the ion exchange chamber 53 is connected to the pen body 51 through threads.

[0059] The color sensor 55 collects the color RGB value presented by the chloride ion concentration of the solution or powder to be tested and transmits it back to the main controller for processing, thereby obtaining the chloride ion concentration of the solution or powder to be tested and displaying the result on the OLED screen 3.

[0060] The color sensor 55 adopts the KV_CORS25516 color sensor with a built-in TCS230 chip. After the color sensor irradiates the object to be measured, the returned light passes through a filter to detect the ratio value of RGB.

[0061] The main controller in the host 1 adopts Raspberry Pi 4. According to the RGB value transmitted back to the main controller by the color sensor 4, the chloride ion concentration is obtained by calculation and the result is output on the OLED screen 2. The result includes four items: R value, G value, B value and concentration.

[0062] The main working process of the detection device includes: pressing the start button to start the device; pressing the detection button, the circuit of the detection pen 5 is turned on, picking up the detection pen and placing the ion exchange chamber 53 into the solution to be tested, the color sensor 55 collects RGB values, and displays the detection results on the OLED screen 3; pressing the reset button to reset the RGB values ​​collected by the color sensor 55 for continuous measurement.

[0063] Example 2

[0064] like Figure 3 and Figure 4 , a method for detecting chloride ions based on a porous anion exchange resin / perovskite nanocrystal multilayer probe, comprising the following steps:

[0065] S1. Preparation of porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin;

[0066] S2. The porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin prepared in S1 is exchanged with a chloride ion solution to obtain the reacted CPB@Resin and the built-in color sensor of the detection pen is used to detect the reacted CPB@Resin to obtain the RGB parameters of multiple sets of three-channel images;

[0067] S3. Use Origin fitting data to establish RGB and C parameters on R, G, B. Cl- Concentration model: C Cl- =kB(RG)+b, where C Cl- is the chloride ion concentration, R, G, B are the values ​​of the red, yellow, and blue color channels respectively, and k and b are coefficients;

[0068] S4. Writing the obtained concentration model into the master controller to form a built-in program;

[0069] S5. Using a chloride ion detection device based on a porous anion exchange resin / perovskite nanocrystal multilayer probe, the chloride ion concentration is calculated through a built-in program and the data is output.

[0070] Example 3

[0071] Cuprous bromide was used to participate in the reaction to prepare a porous anion exchange resin / perovskite nanocrystal multilayer probe.

[0072] The perovskite CsPbBr3 nanocrystalline powder was prepared by hot injection synthesis, which has good stability in water. It was prepared by the following method:

[0073] 1) Add 1.2218g Cs2CO3, 3mL OA, 10mL ODE and 0.03g cuprous bromide to a 100mL glass three-necked flask, and heat at 130-180℃ under vacuum for about 1h until Cs2CO3 is completely dissolved to generate cesium oleate (Cs-OA) with residual cuprous ions. Then, change the vacuum to nitrogen to remove the remaining impurity gases in the system. After 30min, 20mL 0.5mmol / mL Cs-OA solution can be obtained. Transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to 100-150℃ to melt it when it is used;

[0074] 2) Weigh 0.11101 g of lead bromide (PbBr2), pipette 10 mL of ODE, 0.5 mL of OA, and 0.5 mL of OLA, mix and add into a 100 mL three-necked flask, and put in a magnetic stirrer. First, evacuate for 30 min, then heat in a heating mantle at 100-150 ° C under vacuum for 30 min to completely dissolve PbBr2;

[0075] 3) Insert the thermometer into the three-necked flask under nitrogen protection. When the temperature reaches 180°C, use a syringe to absorb 0.2 mL of Cs-OA solution that has been heated and melted in advance, and immediately inject it into the flask. After stirring for 5 seconds, quickly transfer the solution out of the flask and cool it in an ice water bath.

[0076] 4) Add 10 mL of n-hexane and 15 mL of acetone solution to the cooled solution, centrifuge at 11000 rpm, and discard the supernatant in the centrifuge tube;

[0077] 5) After centrifuging the above solution, the solid is placed in a vacuum drying oven for further drying to remove the liquid adsorbed on the solid surface to obtain perovskite CsPbBr3 nanocrystalline powder.

[0078] The anion resin solution was prepared by the following method:

[0079] 20g of chlorine balls (6% DVB, chlorine content 549mmol / g) were swollen with 200ml of dimethylformamide, and then 3 times the amount of tertiary amines (tri-n-butylamine, N-ethylguanidine, N,N-dimethylaniline, trimethylamine) were added. The mixture was left overnight and filtered the next day to obtain an anion resin solution.

[0080] The anion exchange membrane required for preparing the porous anion exchange resin / perovskite nanocrystal multilayer probe comprises the following steps:

[0081] In the anion exchange resin solution, the content of the anion exchange resin is 30wt%, and the anion exchange resin solution is used for scraping to obtain the anion exchange membrane. The scraping temperature is 60°C, and the thickness of the anion exchange membrane is 30nm;

[0082] The porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared as follows:

[0083] The anion exchange membrane is filled at the bottom of the ion exchange chamber, and then the perovskite CsPbBr3 nanocrystal powder is evenly applied on the anion exchange membrane, and finally the anion exchange membrane is filled again to complete the encapsulation, and a porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared. The concentration model is: C Cl - = kB (RG) + b; k = 0.0126; b = 23. Immerse the ion exchange chamber below the test pen in water containing Cl - The wastewater was left to stand for 5 minutes, and the RGB value was measured. The C value was calculated by the concentration model, which was the concentration of chloride ions, 147.9635 ppm. The actual concentration was calculated to be 149 ppm, with an error of 0.6956%.

[0084] Example 4

[0085] Bismuth bromide was used to participate in the reaction to prepare a porous anion exchange resin / perovskite nanocrystal multilayer probe.

[0086] The perovskite CsPbBr3 nanocrystalline powder was prepared by hot injection synthesis, which has good stability in water. It was prepared by the following method:

[0087] 1) Add 1.2218g Cs2CO3, 3mL OA, 10mL ODE and 0.04g bismuth bromide to a 100mL glass three-necked flask, and heat at 130-180℃ under vacuum for about 1h until Cs2CO3 is completely dissolved to generate cesium oleate (Cs-OA) with residual bismuth ions. Then change the vacuum to nitrogen to remove the remaining impurity gas in the system. After 30min, 20mL 0.5mmol / mL Cs-OA solution can be obtained. Transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to 100-150℃ to melt it when it is used;

[0088] 2) Weigh 0.11101 g of lead bromide (PbBr2), pipette 10 mL of ODE, 0.5 mL of OA, and 0.5 mL of OLA, mix and add into a 100 mL three-necked flask, and put in a magnetic stirrer. First, evacuate for 30 min, then heat in a heating mantle at 100-150 ° C under vacuum for 30 min to completely dissolve PbBr2;

[0089] 3) Insert the thermometer into the three-necked flask under nitrogen protection. When the temperature reaches 180°C, use a syringe to absorb 0.2 mL of Cs-OA solution that has been heated and melted in advance, and immediately inject it into the flask. After stirring for 5 seconds, quickly transfer the solution out of the flask and cool it in an ice water bath.

[0090] 4) Add 10 mL of n-hexane and 15 mL of acetone solution to the cooled solution, centrifuge at 11000 rpm, and discard the supernatant in the centrifuge tube;

[0091] 5) After centrifuging the above solution, the solid is placed in a vacuum drying oven for further drying to remove the liquid adsorbed on the solid surface to obtain perovskite CsPbBr3 nanocrystalline powder.

[0092] The anion resin solution was prepared by the following method:

[0093] 20g of chlorine balls (6% DVB, chlorine content 549mmol / g) were swollen with 200ml of dimethylformamide, and then 3 times the amount of tertiary amines (tri-n-butylamine, N-ethylguanidine, N,N-dimethylaniline, trimethylamine) were added. The mixture was left overnight and filtered the next day to obtain an anion resin solution.

[0094] The anion exchange membrane required for preparing the porous anion exchange resin / perovskite nanocrystal multilayer probe comprises the following steps:

[0095] In the anion exchange resin solution, the content of the anion exchange resin is 30wt%, and the anion exchange resin solution is used for scraping to obtain the anion exchange membrane. The scraping temperature is 60°C, and the thickness of the anion exchange membrane is 30nm;

[0096] The porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared as follows:

[0097] The anion exchange membrane is filled at the bottom of the ion exchange chamber, and then the perovskite CsPbBr3 nanocrystal powder is evenly applied on the anion exchange membrane, and finally the anion exchange membrane is filled again to complete the encapsulation, and a porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared. The concentration model is: C Cl - = kB (RG) + b; k = 0.0287; b = 44. Immerse the ion exchange chamber below the test pen in water containing Cl - The wastewater was left to stand for 5 minutes, and the RGB value was measured. The C value was calculated by the concentration model, which was the concentration of chloride ions, 148.0214 ppm. The actual concentration was calculated to be 149 ppm, with an error of 0.6568%.

[0098] Example 5

[0099] Silver bromide was used to participate in the reaction to prepare porous anion exchange resin / perovskite nanocrystal multilayer probes.

[0100] The perovskite CsPbBr3 nanocrystalline powder was prepared by hot injection synthesis, which has good stability in water. It was prepared by the following method:

[0101] 1) Add 1.2218g Cs2CO3, 3mL OA, 10mL ODE and 0.03g silver bromide to a 100mL glass three-necked flask, and heat at 130-180℃ under vacuum for about 1h until Cs2CO3 is completely dissolved to generate cesium oleate (Cs-OA) with residual silver ions. Then, change the vacuum to nitrogen to remove the remaining impurity gas in the system. After 30min, 20mL 0.5mmol / mL Cs-OA solution can be obtained. Transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to 100-150℃ to melt it when it is used;

[0102] 2) Weigh 0.11101 g of lead bromide (PbBr2), pipette 10 mL of ODE, 0.5 mL of OA, and 0.5 mL of OLA, mix and add into a 100 mL three-necked flask, and put in a magnetic stirrer. First, evacuate for 30 min, then heat in a heating mantle at 100-150 ° C under vacuum for 30 min to completely dissolve PbBr2;

[0103] 3) Insert the thermometer into the three-necked flask under nitrogen protection. When the temperature reaches 180°C, use a syringe to absorb 0.2 mL of Cs-OA solution that has been heated and melted in advance, and immediately inject it into the flask. After stirring for 5 seconds, quickly transfer the solution out of the flask and cool it in an ice water bath.

[0104] 4) Add 10 mL of n-hexane and 15 mL of acetone solution to the cooled solution, centrifuge at 11000 rpm, and discard the supernatant in the centrifuge tube;

[0105] 5) After centrifuging the above solution, the solid is placed in a vacuum drying oven for further drying to remove the liquid adsorbed on the solid surface to obtain perovskite CsPbBr3 nanocrystalline powder.

[0106] The anion resin solution was prepared by the following method:

[0107] 20g of chlorine balls (6% DVB, chlorine content 549mmol / g) were swollen with 200ml of dimethylformamide, and then 3 times the amount of tertiary amines (tri-n-butylamine, N-ethylguanidine, N,N-dimethylaniline, trimethylamine) were added. The mixture was left overnight and filtered the next day to obtain an anion resin solution.

[0108] The anion exchange membrane required for preparing the porous anion exchange resin / perovskite nanocrystal multilayer probe comprises the following steps:

[0109] In the anion exchange resin solution, the content of the anion exchange resin is 30wt%, and the anion exchange resin solution is used for scraping to obtain the anion exchange membrane. The scraping temperature is 60°C, and the thickness of the anion exchange membrane is 30nm;

[0110] The porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared as follows:

[0111] like Figure 5 , fill the anion exchange membrane at the bottom of the ion exchange chamber, then evenly apply the perovskite CsPbBr3 nanocrystal powder on the anion exchange membrane, and finally fill the anion exchange membrane again to complete the encapsulation, and prepare a porous anion exchange resin / perovskite nanocrystal multilayer probe. The concentration model is: C Cl - = kB (RG) + b; k = 0.0448; b = 39. Immerse the ion exchange chamber below the test pen in water containing Cl - In the wastewater, the RGB value was measured after standing for 5 minutes. The C value was calculated by the concentration model, which was the concentration of chloride ions, 150.0781 ppm. The actual concentration was calculated to be 149 ppm, with an error of 0.7236%.

[0112] Example 6

[0113] Antimony bromide was used to participate in the reaction to prepare a porous anion exchange resin / perovskite nanocrystal multilayer probe.

[0114] The perovskite CsPbBr3 nanocrystalline powder was prepared by hot injection synthesis, which has good stability in water. It was prepared by the following method:

[0115] 1) Add 1.2218g Cs2CO3, 3mL OA, 10mL ODE and 0.02g silver bromide to a 100mL glass three-necked flask, and heat at 130-180℃ under vacuum for about 1h until Cs2CO3 is completely dissolved to generate cesium oleate (Cs-OA) with residual antimony ions. Then, change the vacuum to nitrogen to remove the remaining impurity gases in the system. After 30min, 20mL 0.5mmol / mL Cs-OA solution can be obtained. Transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to 100-150℃ to melt it when it is used;

[0116] 2) Weigh 0.11101 g of lead bromide (PbBr2), pipette 10 mL of ODE, 0.5 mL of OA, and 0.5 mL of OLA, mix and add into a 100 mL three-necked flask, and put in a magnetic stirrer. First, evacuate for 30 min, then heat in a heating mantle at 100-150 ° C under vacuum for 30 min to completely dissolve PbBr2;

[0117] 3) Insert the thermometer into the three-necked flask under nitrogen protection. When the temperature reaches 180°C, use a syringe to absorb 0.2 mL of Cs-OA solution that has been heated and melted in advance, and immediately inject it into the flask. After stirring for 5 seconds, quickly transfer the solution out of the flask and cool it in an ice water bath.

[0118] 4) Add 10 mL of n-hexane and 15 mL of acetone solution to the cooled solution, centrifuge at 11000 rpm, and discard the supernatant in the centrifuge tube;

[0119] 5) After centrifuging the above solution, the solid is placed in a vacuum drying oven for further drying to remove the liquid adsorbed on the solid surface to obtain perovskite CsPbBr3 nanocrystalline powder.

[0120] The anion resin solution was prepared by the following method:

[0121] 20g of chlorine balls (6% DVB, chlorine content 549mmol / g) were swollen with 200ml of dimethylformamide, and then 3 times the amount of tertiary amines (tri-n-butylamine, N-ethylguanidine, N,N-dimethylaniline, trimethylamine) were added. The mixture was left overnight and filtered the next day to obtain an anion resin solution.

[0122] The anion exchange membrane required for preparing the porous anion exchange resin / perovskite nanocrystal multilayer probe comprises the following steps:

[0123] In the anion exchange resin solution, the content of the anion exchange resin is 30wt%, and the anion exchange resin solution is used for scraping to obtain the anion exchange membrane. The scraping temperature is 60°C, and the thickness of the anion exchange membrane is 30nm;

[0124] The porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared as follows:

[0125] The anion exchange membrane is filled at the bottom of the ion exchange chamber, and then the perovskite CsPbBr3 nanocrystal powder is evenly applied on the anion exchange membrane, and finally the anion exchange membrane is filled again to complete the encapsulation, and a porous anion exchange resin / perovskite nanocrystal multilayer probe is prepared. The concentration model is: C Cl - = kB (RG) + b; k = 0.0335; b = 19. Immerse the ion exchange chamber below the test pen in water containing Cl - The wastewater was left to stand for 5 minutes, and the RGB value was measured. The C value was calculated by the concentration model, which was the concentration of chloride ions, 150.0373 ppm. The actual concentration was calculated to be 149 ppm, with an error of 0.6961%.

[0126] Example 7

[0127] After ion exchange, CPB@Resin can be immersed in Br - After being placed in a solution for 10 minutes, it undergoes secondary ion exchange and can be regenerated into new CPB@Resin. The service life of CPB@Resin is not less than 100 ion cycle exchanges.

[0128] Example 8

[0129] The porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin can adjust the pore size of the anion resin by changing the dosage of dimethylformamide and the swelling time during the swelling process to cope with the influence of various other coexisting ions contained in different chloride ion solutions on the detection, and better protect the CsPbBr3 nanocrystals encapsulated by the anion resin in CPB@Resin.

[0130] Example 9

[0131] The detection device and detection method also include a computer device, which can be a single-chip microcomputer. Its internal structure is as follows Figure 6As shown. The computer device includes a processor, a memory and an external interface connected through a system bus. The processor provides computing and control capabilities. The memory includes a non-volatile storage medium and an internal memory. The non-volatile storage medium stores an operating system, a computer program and a database. The internal memory provides an environment for the operation of the operating system and the computer program. The database is used to store static information and dynamic information data. The network interface of the computer device is used to communicate with an external terminal through a network. When the processor executes the computer program, the steps in the above method embodiment are implemented.

[0132] Those skilled in the art will appreciate that the structure shown in the figure is only a partial structural block diagram related to the solution of the present invention, and does not limit the computer device to which the solution of the present invention is applied. The specific computer device may include more or fewer components than those shown in the figure, or combine certain components, or have a different arrangement of components.

[0133] A computer-readable storage medium is provided, on which a computer program is stored. When the computer program is executed by a processor, the steps in the above method embodiment are implemented.

[0134] Example 10

[0135] The operator moves the chloride ion detection device based on porous anion exchange resin / perovskite nanocrystal multilayer probe to the detection site. After turning on the power, he presses the start button to start the device; presses the detection button to turn on the detection circuit, picks up the detection pen and immerses the ion exchange in the solution to be tested. The sensor module collects RGB values ​​and displays the test results on the OLED screen; presses the reset button to reset the RGB values ​​collected by the color sensor for continuous measurement.

[0136] The present invention utilizes the property that bromide ions in the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin are easy to exchange ions with external chloride ions, and is used as a fluorescent probe in the chloride ion detection device, and the chloride ion concentration data can be obtained quickly and conveniently;

[0137] The present invention utilizes the renewable property of the porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin. The adopted technical solution is low in pollution and non-toxic, which improves the detection safety, reduces the detection cost, and improves the detection accuracy and efficiency. The chloride ion concentration is calculated by the built-in program, and the data can be directly obtained from the screen, which is more intuitive and convenient. Real-time online detection has been realized, which can meet the needs of rapid detection of chloride ions in various scenarios.

[0138] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.

Claims

1. A method for detecting chloride ions based on a porous anion exchange resin / perovskite nanocrystal multilayer probe, characterized in that: The following steps are involved: S1. Preparation of porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin; S2. exchanging the CPB@Resin prepared in S1 with a chloride ion solution to obtain a reacted CPB@Resin, and detecting the reacted CPB@Resin to obtain RGB parameters of multiple groups of three-channel images; S3. Use Origin fitting data to establish RGB and C parameters on R, G, B. Cl- Concentration model: C Cl- =kB(R-G)+b Among them, C Cl- is the chloride ion concentration, R, G, B are the values ​​of the red, yellow, and blue color channels respectively, and k and b are coefficients; S4. Writing the obtained concentration model into the master controller to form a built-in program; S5. Calculate the chloride ion concentration based on the built-in program and output the data.

2. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 1, characterized in that: In S1, the CPB@Resin preparation includes the following steps: S11: Preparation of perovskite CsPbBr3 nanocrystalline powder by hot injection synthesis method; S12: preparing an anion resin solution by an amination scheme; S13: scraping the anion resin solution to obtain an anion exchange membrane; S14: The perovskite CsPbBr3 nanocrystalline powder is evenly applied on the anion exchange membrane and encapsulated to obtain the CPB@Resin.

3. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 2, characterized in that: S11 includes: 1) Add 1-2 g Cs2CO3, 3-10 mL OA, 10-20 mL ODE and 0.01-0.05 g metal compound to a glass three-necked flask, and heat under vacuum until Cs2CO3 is completely dissolved to generate cesium oleate with a small amount of metal remaining; then change the vacuum to nitrogen to remove the remaining impurity gas to obtain 10-30 mL 0.3-0.8 mmol / mL Cs-OA solution, transfer the solution to a glass sample bottle for storage while it is hot, cool it to a solid state at room temperature, and heat it to melt when it is used; 2) Weigh 0.1-0.2 g of lead bromide, pipette 10-20 mL of ODE, 0.5-1.5 mL of OA, and 0.5-1.5 mL of OLA, mix and add into a three-necked flask, add a magnetic stirrer, and heat under vacuum to completely dissolve PbBr2; 3) Insert the thermometer into the three-necked flask under nitrogen protection. After it touches the solution in the flask, heat it up. Use a syringe to absorb 0.1-0.3 mL of Cs-OA solution that has been heated and melted in advance. Immediately inject it into the three-necked flask. After stirring, quickly transfer it out of the three-necked flask and cool it in an ice water bath. 4) Add 5-15 mL of n-hexane and 10-20 mL of acetone solution to the cooled solution, and discard the supernatant in the centrifuge tube after centrifugation; 5) After the above solution is centrifuged, the solid is further dried to remove the liquid adsorbed on the solid surface to obtain perovskite CsPbBr3 nanocrystalline powder.

4. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 3, characterized in that: The metal compound is one or more of cuprous bromide, bismuth bromide, silver bromide and antimony bromide.

5. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 2, characterized in that: The anion resin solution preparation process in S12 is as follows: After 10-30g of chlorine balls are swollen with 150-250mL of dimethylformamide, add 3 times the amount of tertiary amine, leave it overnight, and filter the next day to obtain an anion resin solution.

6. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 2, characterized in that: The thickness of the anion exchange membrane is 10 to 50 nm.

7. The method for detecting chloride ions based on porous anion exchange resin / perovskite nanocrystal multilayer probe according to claim 1, characterized in that: S2 includes the following steps: S21: immersing the CPB@Resin that has not undergone ion exchange in a solution containing chloride ions to obtain the CPB@Resin that has undergone ion exchange; S22: irradiating the ion-exchanged CPB@Resin with an ultraviolet lamp having a wavelength of 280 to 380 nm; S23: Detect the exchanged CPB@Resin to obtain RGB values.

8. A detection device used in the detection method according to any one of claims 1 to 7, characterized in that: The invention comprises a host (1), a mechanical arm (4) and a detection pen (5), wherein the detection pen (5) is fixed to the mechanical arm (4), and an ion exchange chamber (53), an ultraviolet lamp (54) and a color sensor (55) are arranged on the detection pen (5), wherein a porous anion exchange resin / perovskite nanocrystal multilayer probe CPB@Resin is arranged in the ion exchange chamber (53), and the CPB@Resin is formed by evenly applying perovskite CsPbBr3 nanocrystal powder on an anion exchange membrane, the ultraviolet lamp (54) is used to emit ultraviolet light and irradiate the CPB@Resin, and the color sensor (55) is used to detect the RGB value of the light emitted by the CPB@Resin, and transmit the RGB value to the host (1).

9. The detection device according to claim 8, characterized in that: The host (1) is provided with an OLED screen (3).

10. The detection device according to claim 8, characterized in that: A placement rack (6) is fixed at the end of the mechanical arm (4), and the detection pen (5) is fixed on the placement rack (6).