CsPbBr3 (at) PbBr (OH) (at) Ag Raman composite substrate as well as preparation method and application thereof
By coating PbBr(OH) on the surface of CsPbBr3 and recombining it with silver nanoparticles, forming a CsPbBr3@PbBr(OH)@Ag Raman composite substrate, the problem of poor stability of perovskite nanocrystals in water is solved, and the SERS signal is significantly enhanced , the detection effect of 4-mercaptopyrphine has achieved low-cost and efficient detection.
Patent Information
- Application Number
- CN202411255478.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
Perovskite nanocrystals have poor stability in water and are difficult to coexist stably with precious metal nanoparticles. Moreover, their SERS performance has challenges in detecting uniformity and stability in complex environments, especially in CsPbBr3 applications.
Using CsPbBr3@PbBr(OH)@Ag Raman composite substrate, the PbBr(OH) shell layer is coated on the surface of CsPbBr3 and compounded with silver nanoparticles, combined with coating and composite technology, stability is maintained in water, and the preparation method is carried out. Simplify the process and reduce costs.
A CsPbBr3@PbBr(OH)@Ag Raman composite substrate with good stability in water is realized, which significantly enhances the SERS signal, and the detection limit for 4-mercaptopyridine is as low as 17.56 ng/L, with short detection time and low cost, with Wide application potential.
Smart Images

Figure CN119044145A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing perovskite quantum dots by a ligand-assisted recrystallization method and realizing compounding by an in-situ chemical reduction method, as well as application of 4-mercaptopyridine Raman detection, and belongs to the field of nano-luminescent materials and analytical detection. Background Art
[0002] Surface enhanced Raman spectroscopy (SERS) is a basic surface-sensitive technology that enhances Raman scattering by modifying or adsorbing target molecules on a specific surface. It can achieve stable, rapid, label-free and non-destructive detection of various target molecules. Compared with traditional Raman spectroscopy, the SERS effect can amplify the intensity of Raman signals by 10 2 ~10 14 times, greatly broadening the application range of Raman spectroscopy. The application of SERS is highly dependent on the development of SERS substrates, and the manufacturing process of SERS substrates is also constantly improving. At present, commonly used SERS substrates are usually precious metals with rough surfaces such as silver and gold. However, the scarcity and high price of precious metals limit their application, and the research has become mature. The research on SERS active substrates has expanded from metals (Au, Ag and Cu) to semiconductor materials (ZnO, TiO2, etc.).
[0003] Semiconductor nanomaterials have the advantages of being cheap, diverse in nanostructure, adjustable in photoelectric properties, good in chemical stability, and stable in SERS signals. The selective Raman enhancement capability of semiconductor substrates enables their SERS performance to be better utilized in more complex detection environments. However, the SERS performance of semiconductor substrates mainly comes from chemical enhancement, which makes their SERS performance weaker than that of metal substrates. Therefore, compounding semiconductor substrates with metal substrates and synergizing electromagnetic enhancement mechanisms and chemical enhancement mechanisms to obtain better SERS performance has become a new research direction.
[0004] As a semiconductor material, all-inorganic perovskite nanocrystals have the characteristics of adjustable band gap and large dielectric constant. In the substrate composited with silver nanoparticles, they can act as dielectric media to hinder the attenuation of electromagnetic waves in plasma and enhance the electromagnetic field of the substrate. In addition, there is charge transfer at the metal-perovskite interface, and the localized surface plasmon resonance (LSPR) on the metal surface. The synergistic effect of the two promotes SERS enhancement. Therefore, the study of perovskite SERS substrates and their hybrid substrates composited with metal nanoparticles has a good development prospect.
[0005] Perovskite itself is greatly affected by heat, moisture, polar solvents, light exposure and their combined effects. It has poor stability in water, is very easy to decompose, and is difficult to stably coexist with nanoparticles such as Au and Ag. In addition, whether semiconductors as new SERS substrates and hybrid substrates combined with traditional metal nanoparticles can obtain the desired enhanced properties for potential analytes and whether there is a significant enhancement compared to traditional precious metals is a challenge. Finally, the application of CsPbBr3 in SERS detection is in the initial research stage. Ensuring the uniformity and stability of detection in complex environments is an important problem. At the same time, it faces the requirements for the selectivity of the detected objects, which poses many challenges. Summary of the invention
[0006] Object of the invention: The object of the present invention is to provide a CsPbBr3@PbBr(OH)@Ag Raman composite substrate that maintains stability in an aqueous phase; another object of the present invention is to provide a method for preparing a CsPbBr3@PbBr(OH)@Ag Raman composite substrate; another object of the present invention is to provide a.
[0007] Technical solution: The CsPbBr3@PbBr(OH)@Ag Raman composite substrate of the present invention is composed of CsPbBr3@PbBr(OH) and silver nanoparticles. CsPbBr3@PbBr(OH) is composed of CsPbBr3 and a PbBr(OH) shell coated on the surface of CsPbBr3.
[0008] On the other hand, the present invention provides a method for preparing a CsPbBr3@PbBr(OH)@Ag Raman composite substrate, comprising the following steps:
[0009] 1) weighing precursor raw materials, wherein the precursor raw materials are cesium bromide, lead bromide and 2-methylimidazole, and dissolving the precursor raw materials in a mixed solution of N,N-dimethylformamide and methanol to prepare a precursor solution;
[0010] 2) After the precursor solution in step 1) is completely dissolved, oleic acid and oleylamine are added to stabilize the product, and stirred at room temperature;
[0011] 3) filtering the product of step 2), adding toluene solvent to the precipitate, and stirring vigorously to obtain a bright green emitting solution;
[0012] 4) centrifuging, washing and drying the product obtained in step 3) to obtain a CsPbBr3@PbBr(OH) composite material;
[0013] 5) adding the CsPbBr3@PbBr(OH) composite material obtained in step 4) into water and ultrasonicating until uniform, then adding ascorbic acid solution as a reducing agent and sodium citrate solution as a stabilizer, stirring and mixing to obtain a mixed solution;
[0014] 6) Slowly add silver nitrate solution to the mixed solution of step 5) and stir, and finally synthesize the CsPbBr3@PbBr(OH)@Ag Raman composite substrate.
[0015] Furthermore, in step 1), the volume ratio of N,N-dimethylformamide to methanol is 1:1.5-10, wherein the optimal volume ratio is 1:9.
[0016] Furthermore, in step 2), the volume ratio of oleic acid to oleylamine ligand is 1:0.5-1, wherein the optimal volume ratio is 1:0.6.
[0017] Furthermore, in step 5), for every 30 mg of the composite material, the amount of ascorbic acid used is 4-8 mg, and the amount of sodium citrate used is 2-6 mg; preferably, the concentration of the ascorbic acid solution is 4-8 mg / ml, and the amount used is 1 ml; the concentration of the sodium citrate solution is 2-6 mg / ml, and the amount used is 1 ml.
[0018] Furthermore, in step 6), the mass ratio of CsPbBr3@PbBr(OH) to silver nitrate is 15:4; preferably, the concentration of the silver nitrate solution used is 2-6 mg / ml, and the amount used is 2 ml.
[0019] In the above technical solutions, compared with silica and MOF material-coated perovskite quantum dots, the synthesis of rod-shaped PbBr(OH) is simpler and has lower cost.
[0020] On the other hand, the present invention provides an application of the above-mentioned CsPbBr3@PbBr(OH)@Ag Raman composite substrate in detecting 4-mercaptopyridine in water.
[0021] Furthermore, the application method comprises the following steps:
[0022] (1) Aqueous solutions of 4-mercaptopyridine with gradient concentrations were mixed evenly with CsPbBr3@PbBr(OH)@Ag Raman composite substrates, and Raman detection was performed to obtain Raman spectra. The characteristic peak intensity of 4-mercaptopyridine in the spectrum and the concentration of 4-mercaptopyridine were used to construct a linear model to obtain a linear model of 4-mercaptopyridine concentration aqueous solution;
[0023] (2) Using the same conditions as step (1), the test solution and the CsPbBr3@PbBr(OH)@Ag Raman composite substrate are evenly mixed, and Raman detection is performed. The obtained 4-mercaptopyridine characteristic peak intensity is compared with the 4-mercaptopyridine concentration aqueous solution linear model obtained in step (1) to obtain the 4-mercaptopyridine concentration in the test solution.
[0024] Furthermore, the conditions for Raman detection are as follows: the laser power of the Raman spectrometer is 12.5 mW (100%), the wavelength of the excitation light source is 532 nm, and the exposure time is 10 s.
[0025] Further, the linear range of the 4-mercaptopyridine concentration linear model is 0.1-20 μg / L. Specifically, the linear range of the 4-mercaptopyridine concentration linear model is 0.1-20 μg / L, the standard curve equation is y=2917.16x+1398.89, and the correlation coefficient R 2 =0.994, and the detection limit was as low as 17.56 ng / L.
[0026] The preparation method of the present invention is simple, reproducible and low-cost, wherein PbBr(OH) can passivate the surface defect sites of CsPbBr3 nanocrystals in the target product, reduce the influence of instability caused by ion migration, and achieve the purpose of protecting the nanocrystals from interference by the aqueous environment. The substrate prepared by the present invention can be used for Raman enhanced spectroscopy (SERS) detection such as 4-mercaptopyridine, and the SERS signal is significantly enhanced compared with the traditional noble metal substrate, and has good stability in water, uniform dispersion in a sol state, and has application potential.
[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0028] 1) The synthesis method of the present invention is simple to operate and can be carried out at room temperature. It is easy to add a PbBr(OH) framework structure in the preparation method to achieve coating of CsPbBr3 quantum dots, thereby maintaining stability in the aqueous phase;
[0029] 2) The SERS detection effect of the substrate finally synthesized by the present invention on the analyte 4-mercaptopyridine (4-MPY) is much better than that of the pure Ag nanoparticle substrate without composite perovskite;
[0030] 3) This method is simple, efficient, low-cost, has a detection time of less than 10 min, and has a low detection limit, which is conducive to its wide application in SERS detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The SERS spectra of the CsPbBr3@PbBr(OH)@Ag composite substrate prepared in Example 1 for 4-MPY at different concentration gradients;
[0032] Figure 2 The CsPbBr3@PbBr(OH)@Ag composite substrate prepared in Example 1 has different concentration gradients of 4-MPY at 1099±5cm -1 Linear fitting of characteristic peaks at ;
[0033] Figure 3It is the XRD diffraction pattern of CsPbBr3@PbBr(OH);
[0034] Figure 4 This is the SEM image of the CsPbBr3@PbBr(OH) powder prepared in Example 1;
[0035] Figure 5 This is a SEM image of the CsPbBr3@PbBr(OH)@Ag composite substrate prepared in Example 1;
[0036] Figure 6 The composite substrate in Example 2 reacts with different analytes, such as 4-MPY, 4-MBA, 4-ATP and 4-NTP, at 1099 cm -1 Raman intensity histogram.
[0037] Figure 7 The CsPbBr3@PbBr(OH)@Ag composite substrates with different ratios prepared in Examples 1 and 3 are 10 -7 M Comparison of 4-MPY Raman detection;
[0038] Figure 8 The CsPbBr3@PbBr(OH)@Ag composite substrates with different sodium citrate addition amounts prepared in Examples 1 and 4 were 10 -7 M Comparison of 4-MPY Raman detection;
[0039] Fig. 9 The CsPbBr3@PbBr(OH)@Ag composite substrates prepared in Examples 1 and 5 with different ascorbic acid addition amounts were 10 -7 M Comparison of 4-MPY Raman detection;
[0040] Fig.10 For example 1, comparative example 1 and comparative example 2, different substrate pairs 10 -6 M Comparison of 4-MPY Raman detection;
[0041] Fig.11 The CsPbBr3@PbBr(OH)@Ag composite substrates prepared by different methods in Example 1 and Comparative Example 3 are 10 -7 Comparison of M4-MPY Raman detection. DETAILED DESCRIPTION
[0042] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0043] The Raman detection in the examples and comparative examples was performed using a Raman spectrometer with a laser power of 12.5 mW (100%), an excitation light source wavelength of 532 nm, and an exposure time of 10 s.
[0044] Example 1 Preparation of substrate
[0045] The embodiment of the present invention provides a method for preparing a CsPbBr3@PbBr(OH)@Ag Raman composite substrate, comprising the following steps:
[0046] 1) Weigh 1 mmol of cesium bromide, 1.2 mmol of lead bromide and 8 mmol of 2-methylimidazole, and dissolve them in a mixed solution of 1 ml of N,N-dimethylformamide and 9 ml of methanol to prepare a precursor solution;
[0047] 2) After the mixed solution in step 1) is completely dissolved, 1 ml of oleic acid and 0.6 ml of oleylamine are added, and stirred at room temperature for one hour;
[0048] 3) filtering the upper layer solution of step 2), adding 10 ml of toluene solution to the precipitate, and then continuing to stir vigorously for three hours to obtain a bright green emission solution;
[0049] 4) centrifuging the product obtained in step 3), washing it three times with N,N-dimethylformamide and deionized water respectively, and drying it at 40 degrees to obtain CsPbBr3@PbBr(OH) perovskite composite material powder;
[0050] 5) 30 mg of the powder obtained above was added to 60 ml of deionized water and ultrasonicated, then ascorbic acid solution was added as a reducing agent at a concentration of 6 mg / ml, and the amount used was 1 ml; sodium citrate solution was added as a stabilizer at a concentration of 4 mg / ml, and the amount used was 1 ml, and the mixture was stirred for ten minutes;
[0051] 6) Slowly add silver nitrate solution with a concentration of 4 mg / ml and a dosage of 2 ml to the solution in step 5), and gently stir for fifteen minutes to finally synthesize the composite substrate of CsPbBr3@PbBr(OH)@Ag.
[0052] The present invention provides a method for Raman detection of 4-mercaptopyridine, wherein 0.5 ml of the base solution is mixed with 0.5 ml of 4-MPY to be detected with different gradient concentrations, and then the Raman spectroscopy is performed at 1099 ± 5 cm -1 Raman detection was performed on the characteristic peaks.
[0053] like Figure 1 As shown in the figure, it can be seen that this substrate has a good SERS detection effect on the analyte 4-MPY, and can directly detect 10 -9 M. Figure 2 As shown, at 1099±5cm-1 The SERS detection of the characteristic peak has a good linear relationship from 0.1μg / L to 20μg / L, with a linear coefficient of 0.994, and the final detection limit can be calculated to 17.56ng / L.
[0054] XRD characterization analysis
[0055] The product powder (CsPbBr3@PbBr(OH) perovskite composite material powder) synthesized in steps 1)-4) of Example 1 was subjected to XRD analysis. The diffraction peak of the product corresponds to the CsPbBr3 standard card PDF#22-0553, but the peak value is low, due to the addition of less perovskite precursor raw materials and confined growth in PbBr(OH). The other main diffraction peaks of the product correspond to the standard card PDF#30-0697 of PbBr(OH), verifying the successful preparation of CsPbBr3@PbBr(OH).
[0056] SEM characterization analysis
[0057] 1) The morphology of the CsPbBr3@PbBr(OH) powder synthesized in steps 1)-4) of Example 1 was characterized by scanning electron microscopy (SEM). Figure 4 As shown, the tiny brick-shaped plate-like structure of PbBr(OH) can be clearly seen, with a length of about 400-600nm and a width of 200-300nm. At the same time, small spherical particles with a diameter of 300-400nm are generated and there is a phenomenon of adhesion.
[0058] 2) The CsPbBr3@PbBr(OH)@Ag substrate finally synthesized in Example 1 was characterized by SEM, as shown in FIG. Figure 5 As shown, it can be seen that Ag grows on the surface of CsPbBr3@PbBr(OH).
[0059] Example 2 Selectivity Experiment
[0060] Referring to the detection method of Example 1, the concentration of -6 Different types of M-containing thiol-like detection substances 4-mercaptobenzoic acid (4-MBA), 4-aminothiophenol (4-ATP) and 4-nitrothiophenol (4-NTP) were mixed with the SERS substrate at a volume ratio of 1:1 and then Raman detection was performed. Figure 6 As shown, the Raman spectrum at 1099 cm -1 The Raman intensity at the position is plotted as a histogram. It can be seen that the Raman response intensities of other thiol-containing detection objects in this detection system are relatively low, and only 4-MPY shows a high response intensity, indicating that the CsPbBr3@PbBr(OH)@Ag substrate has specific selectivity for 4-MPY.
[0061] Example 3 Optimization of the ratio of perovskite powder to Ag
[0062] The remaining steps were the same as in Example 1, except that the amount of CsPbBr3@PbBr(OH) powder added was changed to 10 mg and 50 mg respectively.
[0063] The synthesized substrates were mixed with 10 -7 M 4-MPY was mixed evenly in a volume ratio of 1:1, and then Raman detection was performed. Figure 7 As shown, it can be seen that the SERS effect is best when 30 mg of perovskite powder is added, and it has the best response intensity.
[0064] Example 4 Optimization of the amount of sodium citrate added as stabilizer
[0065] The remaining steps were the same as in Example 1, except that the amount of sodium citrate added as the stabilizer was changed to 2 mg and 6 mg respectively.
[0066] The synthesized substrates were mixed with 10 -7 M 4-MPY was mixed evenly in a volume ratio of 1:1, and then Raman detection was performed. Figure 8 As shown, it can be seen that when the amount of sodium citrate used is 2-6 mg, there is a better SERS enhancement effect, and when the amount of sodium citrate used is 4 mg, the SERS effect is the best and has the best response intensity.
[0067] Example 5 Optimization of the amount of ascorbic acid added as a reducing agent
[0068] The remaining steps were the same as in Example 1, except that the amount of ascorbic acid added as the reducing agent was changed to 4 mg and 8 mg respectively.
[0069] The synthesized substrates were mixed with 10 -7 M 4-MPY was mixed evenly in a volume ratio of 1:1, and then Raman detection was performed. Fig. 9 As shown, it can be seen that when the amount of sodium citrate used is 4-8 mg, there is a better SERS enhancement effect, and when the amount of sodium citrate used is 6 mg, the SERS effect is the best and has the best response intensity.
[0070] Comparative Example 1
[0071] Referring to the method of Example 1, the synthesized perovskite is directly detected without being compounded with Ag. The specific steps are as follows:
[0072] 1) Weigh 1 mmol of cesium bromide, 1.2 mmol of lead bromide and 8 mmol of 2-methylimidazole, and dissolve them in a mixed solution of 1 ml of N,N-dimethylformamide and 9 ml of methanol to prepare a precursor solution;
[0073] 2) After the mixed solution in step 1) is completely dissolved, 1 ml of oleic acid and 0.6 ml of oleylamine are added, and stirred at room temperature for one hour;
[0074] 3) filtering the upper layer solution of step 2), adding 10 ml of toluene solution to the precipitate, and then continuing to stir vigorously for three hours to obtain a bright green emission solution;
[0075] 4) centrifuging the product obtained in step 3), washing it three times with N,N-dimethylformamide and deionized water respectively, and drying it at 40 degrees to obtain CsPbBr3@PbBr(OH) perovskite composite material powder;
[0076] 5) Take a certain amount of CsPbBr3@PbBr(OH) powder and add it into 10 ml of deionized water, mix it by ultrasonication to form a uniform suspension.
[0077] 6) Take 0.5 ml of the suspension and 0.5 ml of 10 -6 M 4-MPY is mixed with the test substance and then Raman detection is performed.
[0078] Comparative Example 2
[0079] Referring to the method of Example 1, but without adding CsPbBr3@PbBr(OH) powder, a pure nanosilver substrate was prepared, and the specific steps were as follows:
[0080] 1) Take 60 ml of deionized water, then add ascorbic acid solution as a reducing agent, the concentration is 6 mg / ml, the amount used is 1 ml; add sodium citrate solution as a stabilizer, the concentration is 4 mg / ml, the amount used is 1 ml, and stir and mix for ten minutes;
[0081] 2) Slowly add silver nitrate solution with a concentration of 4 mg / ml and a dosage of 2 ml to the solution in step 1), and gently stir for 15 minutes to finally synthesize a pure Ag substrate;
[0082] 3) Take 0.5ml of base solution and 0.5ml of 10 -6 M 4-MPY is mixed with the test substance and then Raman detection is performed.
[0083] like Fig.10 As shown in the comparison of the intensity of the SERS spectrum, the spectrum intensity of Example 1 is about 15.3 times that of the pure nanosilver substrate, and no spectrum signal can be measured for the pure perovskite suspension. This can show that the substrate prepared in Example 1 has the strongest enhanced signal and is suitable for detection. By comparing the three, it can be seen that after the composite perovskite material, the SERS signal is greatly enhanced, which can prove that this CsPbBr3@PbBr(OH)@Ag SERS substrate is very advantageous for the detection of 4-mercaptopyridine.
[0084] Comparative Example 3
[0085] Referring to the synthesis method of patent CN115521784A, another two-step synthesis method was used to prepare CsPbBr3@PbBr(OH) powder. The specific steps are as follows:
[0086] 1) Synthesize a precursor from PbBr2 and 2-methylimidazole. Add 8 mmol of 2-methylimidazole to 9 ml of methanol and stir at room temperature, then dissolve 1.2 mmol of PbBr2 in 1 ml of DMF, add the solution to the methanol solution and stir for one hour to dissolve as much as possible to obtain a precursor solution;
[0087] 2) Replace the mixed solvent of methanol and DMF with 10 ml of toluene of equal volume and poor solubility, take 1 mmol of CsBr and dissolve it in a small amount of water until it is completely dissolved, then slowly add it dropwise to the toluene solution and stir for two hours to obtain a precipitate;
[0088] 3) The precipitate is centrifuged, washed, and dried to obtain light green CsPbBr3@PbBr(OH) powder.
[0089] The remaining steps were the same as in Example 1. CsPbBr3@PbBr(OH)@Ag was synthesized to detect 4-MPY and compared with the substrate prepared in Example 1. Fig.11 It can be seen that the substrate prepared in Example 1 is much better than the substrate prepared by the two-step synthesis method in the existing patent.
[0090] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A CsPbBr3@PbBr(OH)@Ag Raman composite substrate, characterized in that: It is composed of CsPbBr3@PbBr(OH) and silver nanoparticles. CsPbBr3@PbBr(OH) is composed of CsPbBr3 and a PbBr(OH) shell coated on the surface of CsPbBr3.
2. A method for preparing a CsPbBr3@PbBr(OH)@Ag Raman composite substrate, characterized in that: The following steps are involved: 1) weighing precursor raw materials, wherein the precursor raw materials are cesium bromide, lead bromide and 2-methylimidazole, and dissolving the precursor raw materials in a mixed solution of N,N-dimethylformamide and methanol to prepare a precursor solution; 2) After the precursor solution in step 1) is completely dissolved, oleic acid and oleylamine are added to stabilize the product, and stirred at room temperature; 3) filtering the product of step 2), adding toluene solvent to the precipitate, and stirring vigorously to obtain a bright green emitting solution; 4) centrifuging, washing and drying the product obtained in step 3) to obtain a CsPbBr3@PbBr(OH) composite material; 5) adding the CsPbBr3@PbBr(OH) composite material obtained in step 4) into water and ultrasonicating until uniform, then adding ascorbic acid solution as a reducing agent and sodium citrate solution as a stabilizer, stirring and mixing to obtain a mixed solution; 6) Slowly add silver nitrate solution to the mixed solution of step 5) and stir, and finally synthesize the CsPbBr3@PbBr(OH)@Ag Raman composite substrate.
3. The method for preparing the CsPbBr3@PbBr(OH)@Ag Raman composite substrate according to claim 1, characterized in that: In step 1), the volume ratio of N,N-dimethylformamide to methanol is 1:1.5-10.
4. The method for preparing the CsPbBr3@PbBr(OH)@Ag Raman composite substrate according to claim 1, characterized in that: In step 2), the volume ratio of oleic acid to oleylamine ligand is 1:0.5-1.
5. The method for preparing the CsPbBr3@PbBr(OH)@Ag Raman composite substrate according to claim 1, characterized in that: In step 5), for every 30 mg of the composite material, the amount of ascorbic acid used is 4 to 8 mg, and the amount of sodium citrate used is 2 to 6 mg.
6. The method for preparing the CsPbBr3@PbBr(OH)@Ag Raman composite substrate according to claim 1, characterized in that: In step 6), the mass ratio of CsPbBr3@PbBr(OH) to silver nitrate is 15:
4.
7. Use of the CsPbBr3@PbBr(OH)@Ag Raman composite substrate according to claim 1 in detecting 4-mercaptopyridine in water.
8. The use according to claim 7, characterized in that: The application method comprises the following steps: (1) Aqueous solutions of 4-mercaptopyridine with gradient concentrations were mixed evenly with CsPbBr3@PbBr(OH)@Ag Raman composite substrates, and Raman detection was performed to obtain Raman spectra. The characteristic peak intensity of 4-mercaptopyridine in the spectrum and the concentration of 4-mercaptopyridine were used to construct a linear model to obtain a linear model of 4-mercaptopyridine concentration aqueous solution; (2) Using the same conditions as step (1), the test solution and the CsPbBr3@PbBr(OH)@Ag Raman composite substrate are evenly mixed, and Raman detection is performed. The obtained 4-mercaptopyridine characteristic peak intensity is compared with the 4-mercaptopyridine concentration aqueous solution linear model obtained in step (1) to obtain the 4-mercaptopyridine concentration in the test solution.
9. The use according to claim 8, characterized in that: The conditions for Raman detection are as follows: the laser power of the Raman spectrometer is 12.5 mW, the wavelength of the excitation light source is 532 nm, and the exposure time is 10 s.
10. The use according to claim 7, characterized in that: The linear range of the 4-mercaptopyridine concentration linear model was 0.1-20 μg / L.