Mask-free multi-time photoetching micro-nano pattern manufacturing and transferring method
Through the maskless multi-lithography method, combined with laser direct writing and electron beam exposure, the peeling technology is used to solve the problems of low exposure efficiency and dimensional distortion in micro-nano pattern manufacturing, achieving high precision, high efficiency and low cost Pattern transfer, compatible with pattern manufacturing with large and small line widths.
Patent Information
- Application Number
- CN202411368080.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-29
AI Technical Summary
In the manufacturing of complex and refined micro-nano patterns, the prior art has problems with low exposure efficiency, high cost and dimensional distortion after pattern transfer, especially when both micro- and nano-scale lines are included.
The maskless multi-lithography method is used, and the photolithography exposure and coating are carried out in two steps through the combination of laser direct writing and electron beam exposure. The pattern is transferred to the material layer by using peeling technology to avoid dimensional distortion during the etching process.
High-precision, high-efficiency and low-cost micro-nano pattern manufacturing is achieved, and is compatible with patterns with large line widths and small line widths, avoiding the waste of performance during electron beam exposure and the problem of widening size after etching.
Smart Images

Figure CN119045291A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing and transferring a micro-nano pattern, and in particular to a method for manufacturing and transferring a micro-nano pattern by multiple photolithography without a mask. Background Art
[0002] In the semiconductor manufacturing of modern integrated circuits, due to the shrinking of manufacturing nodes and different requirements in various subdivided branches, there is a demand for more complex, refined and diversified nano patterns. For example, the requirements for the shapes of nano columns of different shapes in optical instruments, complex device shapes in MEMS, and resonator interdigitated electrodes in surface acoustic wave devices, etc., in these micro-nano patterns, there will be a situation where the sizes of multiple lines in the pattern are greatly different, such as micron-scale and nanometer-scale lines coexist in the required pattern.
[0003] If only one lithography method is used to make this pattern, such as electron beam exposure technology, its characteristics are high precision, which can often reach 10nm, but its exposure efficiency is very slow. If this refined lithography method is used to make large-area micron-level large-size patterns, it often causes a waste of time and performance. The laser direct writing lithography system is a micron-level lithography system, which is characterized by fast exposure speed and resolution above microns.
[0004] The prior art has a method of using two times of photolithography + etching to transfer patterns. This method uses laser direct writing + etching and electron beam exposure + etching methods. The large line width and small line width patterns in the pattern are photolithographically and etched twice. The photolithography generates the pattern, and the etching achieves the effect of pattern transfer. However, in the photolithography part of this method, if high-precision electron beam exposure is used to make large-size patterns at the micron level, the exposure time will be long and the exposure efficiency will be low due to the problem of electron beam exposure speed, which greatly increases the cost; and in the pattern transfer step after photolithography development, in order to transfer the pattern of the photoresist to a specific material (metal, semiconductor, insulator, etc.), the etching method is used to transfer the pattern, which often causes the line width to become wider after the pattern transfer, that is, the size widening effect, and the distortion after the pattern transfer affects the device performance. Summary of the invention
[0005] Purpose of the invention: The purpose of the invention is to provide a high-precision, high-efficiency, low-cost method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask.
[0006] Technical solution: The method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask of the present invention comprises the following steps:
[0007] (1) using an organic solvent to clean the substrate material, spin-coating a photoresist on the substrate surface, and baking;
[0008] (2) introducing a pattern into a laser direct writing device, performing laser direct writing exposure on a substrate material, and obtaining a pattern larger than 1 micron by exposure; performing development with a developer, removing the exposed photoresist, and obtaining a substrate material after development;
[0009] (3) using a thin film growth method such as electron beam evaporation, magnetron sputtering or atomic layer deposition to coat the developed substrate material to obtain a coated substrate material;
[0010] (4) Soaking the coated substrate material in a water bath of a corrosive solution for heating, separating the substrate material from the film layer, and peeling and transferring the photolithographic pattern to the film layer to obtain a pattern above the micrometer level;
[0011] (5) spin coating a photoresist on the surface of the substrate material separated in step (4) and baking;
[0012] (6) introducing a pattern into an electron beam exposure device, and performing electron beam exposure on the substrate material in alignment with the overlay mark to obtain a pattern with a line width of less than 1 micron; performing development with a developer to remove the exposed photoresist and obtain a substrate material after secondary development;
[0013] (7) using a thin film growth method selected from electron beam evaporation, magnetron sputtering or atomic layer deposition to coat the substrate material after secondary development to obtain a substrate material after secondary coating;
[0014] (8) The substrate material after the secondary coating is immersed in a corrosive solution and heated in a water bath to separate the substrate material and the film layer, and the photolithography pattern is peeled off and transferred to the film layer to obtain a nanoscale pattern.
[0015] Wherein, in step (1), the organic solvent cleaning is to place it in acetone and isopropanol in sequence for ultrasonic cleaning for 5 to 10 minutes, the photoresist is a photosensitive photoresist, and the substrate material is a silicon semiconductor or silicon oxide with a conductive film, or a sapphire insulator; the spin coating is specifically to use an initial rotation speed of 500 to 700 rpm for 5 to 10 seconds, and a subsequent rotation speed of 1000-5000 rpm for 30 to 40 seconds; the baking temperature is 100 to 180° C., and the time is 70 to 120 seconds, preferably 90 seconds.
[0016] Wherein, in step (2), the exposure dose is 10-100 mJ / cm 2 ; The developer is a photosensitive photoresist developer, and the developing time is 25 to 45 seconds.
[0017] Among them, in step (3), the coating film, its film material is one of metal, semiconductor or insulator; specifically, other semiconductor materials such as polysilicon, single crystal silicon, etc., or other insulating materials such as silicon oxide, silicon nitride, etc., or other metal materials such as titanium, gold, etc., and the material layer can also be a single layer or multiple layers.
[0018] Wherein, in step (5), the photoresist is an electron beam photoresist; the spin coating is specifically performed by using an initial rotation speed of 500-700 rpm for 5-10 seconds and a subsequent rotation speed of 1000-5000 rpm for 30-40 seconds; the baking temperature is 160-180°C and the time is 70-120 seconds, preferably 90 seconds.
[0019] Wherein, in step (6), the exposure dose is 100-500uC / cm 2 ; The developer is an electron beam photoresist developer, and the developing time is 90 to 150 seconds; preferably 120 seconds.
[0020] Wherein, in step (4) or (8), the etching solution is one of acetone or N-methylpyrrolidone solution, and the water bath heating is performed at a temperature of 50 to 70° C. for 2 to 24 h, preferably at 70° C. for 12 h.
[0021] Principle of the invention: The present invention proposes a technology of performing two photolithography exposures and stripping for patterns with different line widths in micro-nano manufacturing to solve this problem. The pattern is divided into two layers, one above 1 micron and one below 1 micron, and the classification can be performed using the format of a GDS file. In the first step, a laser direct writing photolithography method is used to manufacture a pattern above 1 micron, and then a stripping method is used to manufacture the required part of the micron patterned material. In the second step, an electron beam exposure method is used for overlay, exposing a pattern below 1 micron, and electron beam evaporation and stripping are performed to manufacture the remaining part of the nano-patterned material. The present invention adopts photolithography exposure followed by film coating, and finally adopts a stripping method for photolithography pattern transfer, which can perfectly avoid the problem of poor pattern transfer effect caused by etching the photolithography pattern. At the same time, the present invention adopts the method of laser direct writing exposure + electron beam exposure, which does not require a photolithography mask, and can reduce the manufacturing cost and the exposure error caused by the photolithography plate.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0023] (1) The double exposure plus stripping method can accommodate both large line width (above micrometer level) and small line width (nanometer level) in the pattern, thus avoiding the performance waste when exposing large-area and large-size patterns using electron beam exposure; (2) The preparation process does not require a photolithography mask, which is low in cost and overcomes the exposure error of the photolithography plate, while avoiding distortion after the etched pattern is transferred. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a brief flow chart of the present invention;
[0025] Figure 2 A planar pattern designed for the method of the present invention;
[0026] Figure 3 An actual plan view of a micro-nano pattern obtained according to an embodiment of the present invention;
[0027] Figure 4 This is a cross-sectional view of a micro-nano pattern obtained according to an embodiment of the present invention. DETAILED DESCRIPTION
[0028] The technical scheme of the present invention is further described below in conjunction with the examples. The test materials used in the examples can all be purchased through conventional channels.
[0029] Example 1
[0030] A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask specifically comprises the following steps:
[0031] In terms of pattern design, the pattern lines should be divided into two parts: above 1 micron and below 1 micron. Here, the pattern part larger than 1 micron is called micron pattern, and the pattern smaller than 1 micron is called nano pattern. Figure 2 As shown, it is an example of the classification method involved in the present invention, wherein the pattern outside the black frame is pattern one, with a line width greater than 1 micron, and the pattern inside the black frame is pattern two, with a line width less than 1 micron; after designing the two parts of the pattern, an electron beam alignment mark is added to facilitate subsequent overlay.
[0032] (1) In terms of sample preparation, the following steps were completed at room temperature unless otherwise specified:
[0033] The substrate material is organically cleaned, and the substrate material is sapphire with a conductive film. The samples are placed in acetone and isopropanol for ultrasonic cleaning for about 5 minutes to remove impurities on the surface. Then the samples are placed in a photoresist and evacuated. AZ series photoresists are used, including positive and negative photoresists, specifically AZ5214 photoresists. The photoresist is sucked into a dropper and dripped on the sample. The initial speed of 500 rpm is used for photoresisting for 5 seconds, and the final speed of 4000 rpm is used for photoresisting for 30 seconds. After the photoresist is spin-coated, the sample is placed on a hot plate and baked at 100°C for about 90 seconds to remove the solvent in the photoresist and achieve a solid film effect.
[0034] (2) Place the sample in a laser direct writing device, specifically, Microwriter ML3. Import the GDS format file with the micrometer-level pattern design into the device and convert the data into a format file that can be read by the laser direct writing device. Then, use 30mJ / cm 2 After exposure, the sample is taken out of the device and placed in a developer of AZ series photoresist, specifically 3038 developer (a mixed solution of 2.38% tetramethylammonium hydroxide and water). After developing in the developer for 30 seconds, the sample is placed in deionized water to remove the residual developer to achieve a fixing effect.
[0035] (3) The sample with the photolithography pattern is placed in a coating device to grow a material layer. 50nmTi+100nmAu is deposited on the material using electron beam evaporation to coat a layer of material on the photolithography sample.
[0036] (4) Place the sample in a 70°C water bath and heat acetone for 12 hours to remove the material on the photoresist. After that, only the material layer without the photoresist in the exposed area remains, and the first part of the micron pattern is transferred to the material layer.
[0037] (5) Then, the sample is placed in a coating machine and evacuated. The PMMA series / ZEP series electron beam photoresist, specifically PMMA A2 electron beam photoresist, is used. The electron beam photoresist is sucked into a dropper and dripped on the sample. The initial speed is 500 rpm for 5 seconds, and the final speed is 2000 rpm for 30 seconds. The sample is then placed on a hot plate at 180°C and baked for about 90 seconds to remove the solvent in the electron beam photoresist and achieve a solid film effect.
[0038] (6) Place the sample in an electron beam exposure device, specifically a Raith EBL device. Import the GDS format file with the nanoscale pattern design into the device and convert the data into a format file that can be read by the electron beam exposure device. Then, after alignment using the overlay mark, use an acceleration voltage of 20 keV and 220 uC / cm 2 After exposure with a dose of , the sample is taken out of the device, placed in a developer of PMMA series photoresist (a solution of tetramethyl dipentyl ketone and isopropyl alcohol in a ratio of 1:3) for 120 seconds, and then placed in isopropyl alcohol to remove the residual developer to achieve a fixing effect and form a nanoscale pattern.
[0039] (7) The sample with the photolithography pattern is placed in a coating device to grow a material layer. 50nmTi+100nmAu is deposited on the material using electron beam evaporation to coat a layer of material on the photolithography sample.
[0040] (8) The sample is placed in a 70°C water bath and heated with acetone for 12 hours to remove the material on the photoresist, as used in the present invention. After that, only the material layer without the photoresist portion in the exposed area remains, and the second part of the nanopattern is transferred to the material layer.
[0041] Example 2
[0042] A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask. Compared with Example 1, the substrate material in step (1) is changed to a silicon semiconductor, and finally the method can complete the manufacturing and transfer of micro-nano patterns by multiple photolithography without a mask with high precision, high efficiency and low cost.
[0043] Example 3
[0044] A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask. Compared with Example 1, the thin film growth method in step (3) is changed to a thin film growth method by magnetron sputtering, which can ultimately complete the manufacturing and transfer of micro-nano patterns by multiple photolithography without a mask with high precision, high efficiency and low cost.
[0045] Example 4
[0046] A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask. Compared with Example 1, the photoresist structure in step (1) is changed from one layer of photoresist to two layers of photoresist, wherein the newly added layer of photoresist is thinner and more sensitive to increase the fault tolerance of stripping.
[0047] Example 5
[0048] A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask. Compared with Example 1, the number of electron beam photoresist layers in step (3) is changed from one electron beam photoresist layer to an electron beam photoresist layer, wherein the newly added electron beam photoresist layer is thinner and has a higher sensitivity, so as to increase the fault tolerance of stripping.
[0049] like Figure 3 As shown, it is a plan view of the micro-nano pattern obtained in Example 1, and Figure 2 In contrast, the pattern produced is similar to the design plate during photolithography. Figure 1 The pattern edges are clear and steep, and the line width is consistent with the photolithographic pattern, completely restoring the design layout.
[0050] like Figure 4 The cross-sectional view of the micro-nano pattern is shown. It can be seen that the material is very steep, and there is no material tilt angle compared to the etching method. The steep pattern produced by this method has a very positive effect on the propagation performance of the surface acoustic wave resonator, such as Q value, electromechanical coupling coefficient, etc. It will also have a very good effect on the performance of MEMS devices and optical waveguide devices.
[0051] Therefore, according to the nanoscale fine pattern processing method of the present invention, laser direct writing exposure and electron beam exposure are performed for patterns above 1 micron and patterns below 1 micron respectively, so that nanoscale fine patterns can be processed quickly and at low cost, and the stripping method is used to transfer the photolithography pattern to the material layer, which can avoid the line width loss caused by etching and can perform pattern transfer more accurately.
Claims
1. A method for manufacturing and transferring micro-nano patterns by multiple photolithography without a mask, characterized in that: The following steps are involved: (1) using an organic solvent to clean the substrate material, spin-coating a photoresist on the substrate surface, and baking; (2) introducing a pattern into a laser direct writing device, performing laser direct writing exposure on a substrate material, and obtaining a pattern larger than 1 micron by exposure; Using a developer to perform development, removing the exposed photoresist, and obtaining a developed substrate material; (3) using a thin film growth method such as electron beam evaporation, magnetron sputtering or atomic layer deposition to coat the developed substrate material to obtain a coated substrate material; (4) Soaking the coated substrate material in a water bath of an etchant to heat it, separating the substrate material from the film layer, and peeling off and transferring the photolithography pattern to the film layer to obtain a pattern above the micrometer level; (5) spin coating a photoresist on the surface of the substrate material separated in step (4) and baking; (6) introducing a pattern into an electron beam exposure device, and performing electron beam exposure on the substrate material in alignment with the overlay mark to obtain a pattern with a line width of less than 1 micron; Using a developer to develop, remove the exposed photoresist, and obtain a substrate material after secondary development; (7) using a thin film growth method selected from electron beam evaporation, magnetron sputtering or atomic layer deposition to coat the substrate material after secondary development to obtain a substrate material after secondary coating; (8) The substrate material after the secondary coating is immersed in a corrosive solution and heated in a water bath to separate the substrate material and the film layer, and the photolithography pattern is peeled off and transferred to the film layer to obtain a nanoscale pattern.
2. The method according to claim 1, characterized in that: In step (1), the organic solvent cleaning is to place the sample in acetone and isopropanol for ultrasonic cleaning for 5 to 10 minutes in sequence, the photoresist is a photosensitive photoresist, and the substrate material is a silicon semiconductor or silicon oxide with a conductive film, or a sapphire insulator.
3. The method according to claim 1, characterized in that In step (2), the developer dosage is 10-100 mJ / cm 2 ; The developer is a photosensitive photoresist developer, and the developing time is 25 to 45 seconds.
4. The method according to claim 1, characterized in that: In step (3), the coating is made of a material selected from the group consisting of metal, semiconductor and insulator.
5. The method according to claim 1, characterized in that In step (5), the photoresist is electron beam photoresist.
6. The method according to claim 1, characterized in that In step (6), the developer dosage is 100-500uC / cm 2 ; The developer is an electron beam photoresist developer, and the developing time is 90 to 150 seconds.
7. The method according to claim 1, characterized in that In step (1) or (5), the spin coating is specifically performed by using an initial rotation speed of 500-700 rpm for 5-10 seconds and a subsequent rotation speed of 1000-5000 rpm for 30-40 seconds; the baking temperature is 160-180°C and the time is 70-120 seconds.
8. The method according to claim 1, characterized in that In step (4) or (8), the etching solution is one of acetone or N-methylpyrrolidone solution, and the water bath heating is performed at a temperature of 50 to 70° C. for a time of 2 to 24 hours.
Citation Information
Patent Citations
Mixing line making method
CN102983066A
Manufacturing method for hybrid lines
CN103187246A
Nano fine-patterning processing method
CN104597724A
Preparation method and preparation system of micro-nano pattern
CN107555396A
Self-supported micro-nano structure and manufacturing method thereof
CN109437093A
Cited By
Preparation method of binary photomask and binary photomask
CN119439607A
Multistage fine overlay method for complex micro-nano structure
CN121578592A
A multi-stage fine overlay method for complex micro-nano structures
CN121578592B
Photoetching direct-writing micro-nano machining equipment and machining method
CN121995710A