Micro-LED chip preparation method based on cavity patterned substrate
By introducing cavity microstructure and patterned ITO layer into the interface of the sapphire substrate and AlN buffer layer of the Micro-LED chip, the problem of low optical output power of the chip is solved and the photoelectric performance is improved.
Patent Information
- Application Number
- CN202411092764.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-29
AI Technical Summary
The bottom transparent sapphire substrate of the Micro-LED chip prepared based on Group III-V inorganic materials has low efficiency in reflecting light emitted in the active region, limiting the photoelectric performance of the chip, especially the frontal light output power.
The cavity microstructure was introduced at the interface of the patterned sapphire substrate and the AlN buffer layer, trenches were formed by nanosecond pulsed laser scanning etching and thermochemical corrosion, and the patterned ITO layer was evaporated on the p-GaN surface to reduce light Absorption loss.
The front light output power of the Micro-LED chip is improved, the photoelectric performance of the chip is improved, and the light is reflected through the cavity microstructure and redirected to the escape cone, reducing the light absorption loss.
Smart Images

Figure CN119050209A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor device technology, and in particular to a method for preparing a Micro-LED chip based on a cavity patterned substrate. Background Art
[0002] Micro-LEDs based on III-V inorganic materials have performance advantages such as long life, high brightness and low power consumption, and are suitable for intelligent mobile terminal display fields such as virtual reality, augmented reality (AR), mixed reality, micro-projection and visual display. However, for the horizontally structured Micro-LED chips, the transparent sapphire substrate at the bottom has low reflection efficiency for the light emitted from the active area, which seriously limits the light extraction efficiency of the top of the Micro-LED chip, further restricting the optoelectronic performance of the Micro-LED chip.
[0003] Therefore, how to increase the front light output power of Micro-LED is an urgent problem to be solved. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention proposes a method for preparing a Micro-LED chip, which includes preparing a cavity microstructure introduced at the interface of a patterned sapphire substrate and an AlN buffer layer using nanosecond pulse laser scanning etching and thermochemical etching technology. The cavity microstructure reflects and redirects the emitted light to the escape cone at the top of the Micro-LED chip, thereby increasing the light output power at the top of the chip. At the same time, a patterned ITO layer is evaporated on the p-GaN surface to reduce the absorption loss of the emitted light. The present invention enhances the front light output power of the Micro-LED chip and improves the optoelectronic performance of the chip.
[0005] In one aspect of the present invention, the present invention provides a method for preparing a Micro-LED chip. According to an embodiment of the present invention, the method comprises:
[0006] 1) Providing an epitaxial wafer, comprising a substrate and an epitaxial layer, wherein the epitaxial layer comprises an AlN buffer layer, an n-GaN layer, an active region layer, a p-AlGaN electron blocking layer and a p-GaN layer;
[0007] 2) depositing a SiO2 protective layer on the surface of the p-GaN layer;
[0008] 3) Scanning and etching the epitaxial layer using nanosecond pulse laser to form a groove;
[0009] 4) etching the groove by thermal chemical etching to form a cavity microstructure near the groove area at the interface between the substrate and the AlN buffer layer;
[0010] 5) removing the SiO2 protective layer in step 2), introducing an ITO layer, and etching the ITO layer to form a patterned ITO layer;
[0011] 6) Depositing a SiO2 passivation layer on the patterned ITO layer, and vapor-depositing a p-electrode and an n-electrode on the SiO2 passivation layer to form the Micro-LED chip. According to the method of the embodiment of the present invention, a cavity microstructure is introduced at the interface between the substrate and the AlN buffer layer, and the cavity microstructure reflects and redirects the emitted light to the escape cone at the top of the Micro-LED chip, thereby increasing the light output power at the top of the chip. At the same time, vapor-depositing a patterned ITO layer on the p-GaN surface reduces the absorption loss of the emitted light. The Micro-LED chip prepared by the method of the embodiment of the present invention enhances the front light output power of the Micro-LED chip and improves the optoelectronic performance of the chip.
[0012] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0013] According to an embodiment of the present invention, the epitaxial layer is formed by sequentially growing an AlN buffer layer, an n-GaN layer, an active region layer, a p-AlGaN electron blocking layer and a p-GaN layer on the substrate by metal organic chemical vapor deposition technology.
[0014] According to an embodiment of the present invention, the substrate is a patterned sapphire substrate.
[0015] According to an embodiment of the present invention, the patterned sapphire substrate is a sapphire substrate having a periodic conical sapphire or SiO2 array on the surface.
[0016] According to an embodiment of the present invention, the height of the cavity microstructure is 3-5 μm, such as 3 μm, 4.3 μm and 4.6 μm.
[0017] According to an embodiment of the present invention, depositing a SiO2 protective layer on the surface of the p-GaN layer is performed by plasma enhanced chemical vapor deposition technology.
[0018] According to an embodiment of the present invention, the wavelength of the nanosecond pulse laser is 355 nm. The inventors have found that common pulse laser wavelengths include 355 nm, 532 nm and 1064 nm, etc. Short-wavelength lasers have greater energy and higher etching efficiency for materials.
[0019] According to an embodiment of the present invention, the repetition frequency of the nanosecond pulse laser is 20-100 kHz.
[0020] According to an embodiment of the present invention, the output power of the nanosecond pulse laser is 0.1-2W.
[0021] According to an embodiment of the present invention, the width of the groove is 2-6 μm.
[0022] According to an embodiment of the present invention, the solution used for the thermal chemical etching is a mixed solution of H3PO4 and H2SO4, which is a commonly used mixed solution for etching AlN materials.
[0023] According to an embodiment of the present invention, the ratio of the mixed solution of H3PO4 and H2SO4 is 3 to 1. The inventors found that the ratio of the mixed solution directly affects the size of the etched cavity microstructure, and the size of the cavity microstructure affects the light reflection efficiency. Under this ratio, the size of the etched cavity microstructure is appropriate.
[0024] According to an embodiment of the present invention, the thermochemical etching temperature is 200-300° C. The inventors found that the etching temperature directly affects the size of the etched cavity microstructure, and the size of the cavity microstructure affects the light reflection efficiency. At this temperature, the size of the etched cavity microstructure is appropriate.
[0025] According to an embodiment of the present invention, the thermochemical etching time is 1 to 30 minutes. The inventors found that the etching time directly affects the size of the etched cavity microstructure, and the size of the cavity microstructure affects the light reflection efficiency. Under this time, the height of the etched cavity microstructure is appropriate.
[0026] According to an embodiment of the present invention, the thermochemical etching time is less than 15 minutes. The inventors found that under this time, the height of the etched cavity microstructure is more appropriate.
[0027] According to an embodiment of the present invention, the thermochemical etching time is less than 10 minutes. The inventors found that under this time, the height of the etched cavity microstructure is more appropriate.
[0028] According to an embodiment of the present invention, the thermochemical etching time is 5 minutes. The inventors found that under this time, the height of the etched cavity microstructure is more suitable. According to an embodiment of the present invention, the removal of the SiO2 protective layer in step 2) is performed by wet etching technology.
[0029] According to an embodiment of the present invention, the etching of the ITO layer to form a patterned ITO layer further comprises etching the epitaxial layer by photolithography and dry etching techniques until the p-GaN layer is exposed. According to an embodiment of the present invention, the patterned ITO layer is to etch the ITO layer to form a circular hole array in the ITO layer.
[0030] According to an embodiment of the present invention, before evaporating the p-electrode and the n-electrode on the SiO2 passivation layer, the method further includes etching the p-through hole and the n-through hole on the SiO2 passivation layer respectively by using photolithography and dry etching technology.
[0031] In another aspect of the present invention, the present invention further proposes a method for preparing a Micro-LED chip based on a cavity patterned substrate. According to an embodiment of the present invention, the method comprises:
[0032] Step 1: using metal organic chemical vapor deposition (MOCVD) technology to sequentially grow an AlN buffer layer, an n-GaN layer, an active region layer, a p-AlGaN electron blocking layer and a p-GaN layer on a patterned sapphire substrate to form an epitaxial layer;
[0033] Step 2: Depositing a SiO2 protective layer on the surface of p-GaN using plasma enhanced chemical vapor deposition (PECVD) technology;
[0034] Step 3: Use nanosecond pulse laser to perform rectangular path scanning etching on the epitaxial wafer to form a groove;
[0035] Step 4: etching the groove by thermal chemical etching to form a cavity microstructure near the groove area at the interface between the patterned sapphire substrate and the AlN buffer layer;
[0036] Step 5: Use wet etching technology to remove the SiO2 protective layer on the surface of p-GaN, then evaporate an ITO layer as a current spreading layer, and use photolithography and dry etching technology to etch the epitaxial layer until the p-GaN layer is exposed. Etch the ITO layer to form a patterned ITO layer, and then deposit a SiO2 passivation layer;
[0037] Step 6: Use photolithography and dry etching technology to etch p-through holes and n-through holes on the SiO2 passivation layer respectively, and then evaporate p-electrode and n-electrode respectively to form Micro-LED.
[0038] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0039] According to an embodiment of the present invention, in the step 1, the patterned sapphire substrate is a sapphire substrate having a periodic conical sapphire or SiO2 array on the surface.
[0040] According to an embodiment of the present invention, in step 3, the wavelength of the nanosecond pulse laser is 355 nm, the repetition frequency is 20-100 kHz, and the laser output power is 0.1-2 W. The width of the etched groove is 2-6 μm.
[0041] According to an embodiment of the present invention, in step 4, the solution used for the thermal chemical etching is a mixed solution of H3PO4 and H2SO4 in a ratio of 3 to 1, the etching temperature is 200 to 300° C., and the etching time is 1 to 30 minutes.
[0042] According to an embodiment of the present invention, in step five, the patterned ITO layer is evenly distributed with a circular hole array prepared by photolithography and wet etching processes.
[0043] In another aspect of the present invention, the present invention further provides a Micro-LED chip. According to an embodiment of the present invention, the Micro-LED chip is prepared by the method described above.
[0044] According to the embodiments of the present invention, the present invention has at least one of the following beneficial effects:
[0045] 1) The present invention introduces a cavity microstructure at the interface of the patterned sapphire substrate and the AlN buffer layer by nanosecond pulse laser scanning etching and thermal chemical etching technology.
[0046] 2) The cavity microstructure reflects and redirects the emitted light to the escape cone at the top of the Micro-LED chip, increasing the light output power at the top of the chip.
[0047] 3) The patterned ITO layer on the top can reduce the absorption loss of the emitted light and further improve the optoelectronic performance of the Micro-LED chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0049] Figure 1 A flow chart showing a method for preparing a Micro-LED chip based on a cavity patterned substrate in an embodiment of the present invention is shown;
[0050] Figure 2 A schematic diagram of the epitaxial layer structure in an embodiment of the present invention is shown;
[0051] Figure 3 A schematic diagram of the epitaxial layer structure after depositing a SiO2 protective layer in an embodiment of the present invention is shown;
[0052] Figure 4A schematic diagram of the epitaxial layer structure after laser scanning and etching of grooves in an embodiment of the present invention is shown;
[0053] Figure 5 A top view of the epitaxial layer after the grooves are etched by laser scanning in an embodiment of the present invention is shown;
[0054] Figure 6 A schematic diagram of the epitaxial layer structure after thermochemical etching in an embodiment of the present invention is shown;
[0055] Figure 7 A schematic diagram of the epitaxial layer structure after removing the SiO2 protective layer in an embodiment of the present invention is shown;
[0056] Figure 8 A schematic diagram of the epitaxial layer structure after the ITO layer is deposited in an embodiment of the present invention is shown;
[0057] Fig. 9 A schematic diagram of the epitaxial layer structure after Mesa etching in an embodiment of the present invention is shown;
[0058] Fig.10 A schematic diagram of the epitaxial layer structure after the ITO layer is patterned in an embodiment of the present invention is shown;
[0059] Fig.11 A top view of a patterned ITO layer in an embodiment of the present invention is shown;
[0060] Fig.12 A schematic diagram of the structure of an epitaxial wafer after a SiO2 passivation layer is deposited in an embodiment of the present invention is shown;
[0061] Fig.13 A schematic diagram of the epitaxial layer structure after the electrode is evaporated in an embodiment of the present invention is shown;
[0062] Fig.14 A light output comparison diagram of an embodiment of the present invention and a comparative example is shown;
[0063] Description of reference numerals:
[0064] 101. Patterned sapphire substrate; 102. AlN buffer layer; 103. n-GaN layer; 104. Active region layer; 105. p-AlGaN electron blocking layer; 106. p-GaN layer; 107. SiO2 protective layer; 108. Groove; 109. Cavity microstructure; 110. ITO layer; 111. Patterned ITO layer; 112. SiO2 passivation layer; 113. Electrode. DETAILED DESCRIPTION
[0065] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0066] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0067] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0068] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0069] Example
[0070] like Figure 1 As shown, one embodiment of the present invention provides a method for preparing a Micro-LED chip based on a cavity patterned substrate, comprising the following steps:
[0071] S101, using MOCVD technology to sequentially grow an AlN buffer layer 102, an n-GaN layer 103, an active region layer 104, a p-AlGaN electron blocking layer 105 and a p-GaN layer 106 on a patterned sapphire substrate 101 to form an epitaxial wafer, such as Figure 2 As shown in Figure 1, the patterned sapphire substrate has a periodic array of cones on its surface.
[0072] S102, using PECVD technology to deposit a 2 μm thick SiO2 protective layer 107 on the surface of p-GaN 106, such as Figure 3 shown.
[0073] S103, using nanosecond pulse laser to perform rectangular path scanning etching on the epitaxial wafer to form a groove 108, such as Figure 4 The top view of the groove 108 is shown in Figure 5As shown. The wavelength of the nanosecond pulse laser is 355nm, the repetition frequency is 50kHz, and the laser output power is 0.8W. The width of the etched groove is 4μm.
[0074] S104, the groove 108 is etched by thermal chemical etching. Since the dislocation density at the interface between the patterned sapphire substrate 101 and the AlN buffer layer 102 is high and the crystal quality is poor, the mixed solution of H3PO4 and H2SO4 flowing from the groove will selectively etch the defects in the area, forming a cavity microstructure 109 between the patterned sapphire substrate 101 and the AlN buffer layer 102, as shown in FIG. Figure 6 As shown in Figure 2, the height of the cavity microstructure is 3 μm. The mixing ratio of H3PO4 and H2SO4 is 3:1, the etching temperature is 250°C, and the etching time is 5 minutes.
[0075] S105, using wet etching technology to remove the SiO2 protective layer 107 on the surface of the p-GaN layer 106, such as Figure 7 Then, an ITO layer 110 is evaporated on the surface of the p-GaN layer 106 as a current spreading layer, as shown in FIG. Figure 8 The epitaxial wafer is etched using photolithography and dry etching techniques until the n-GaN layer 103 is exposed, as shown in FIG. Fig. 9 Then the ITO layer 110 is etched into a patterned ITO layer 111 having a circular hole array distribution, as shown in FIG. Fig.10 As shown, the top view of the patterned ITO layer 111 is as shown Fig.11 shown.
[0076] S106, depositing a SiO2 passivation layer 112 on the surface of the epitaxial wafer, such as Fig.12 Subsequently, p-through holes and n-through holes are etched on the SiO2 passivation layer by photolithography and dry etching techniques, and Cr / Al / Ti / Pt / Au metal is evaporated as the electrode 113 to form a Micro-LED chip based on a cavity patterned substrate.
[0077] The difference between Comparative Example 1 and the embodiment is that there is no cavity microstructure.
[0078] Comparative Examples 2-3 are basically the same as the embodiment, and the thermochemical etching time is 10 minutes and 15 minutes respectively. The thermochemical etching time will affect the height of the cavity microstructure. The height of the cavity microstructure of Comparative Examples 2 and 3 is 4.3 μm and 4.6 μm respectively.
[0079] The output power of the Micro-LED chip arrays prepared in the embodiment and comparative examples 1 to 3 was tested. The results are as follows: Fig.14As shown. It can be seen that thanks to the more suitable size of the cavity microstructure, more light emitted from the active area is reflected to the top of the Micro-LED chip, and the embodiment shows the maximum light output power.
[0080] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0081] The above description is only a preferred specific implementation manner of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention should be included in the scope of protection of the invention.
[0082] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0083] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a Micro-LED chip, characterized in that: include: 1) Providing an epitaxial wafer, comprising a substrate and an epitaxial layer, wherein the epitaxial layer comprises an AlN buffer layer, an n-GaN layer, an active region layer, a p-AlGaN electron blocking layer and a p-GaN layer; 2) depositing a SiO2 protective layer on the surface of the p-GaN layer; 3) Scanning and etching the epitaxial layer using nanosecond pulse laser to form a groove; 4) etching the groove by thermal chemical etching to form a cavity microstructure near the groove area at the interface between the substrate and the AlN buffer layer; 5) removing the SiO2 protective layer in step 2), introducing an ITO layer, and etching the ITO layer to form a patterned ITO layer; 6) Depositing a SiO2 passivation layer on the patterned ITO layer, and evaporating a p-electrode and an n-electrode on the SiO2 passivation layer to form the Micro-LED chip.
2. The method according to claim 1, characterized in that: The epitaxial layer is formed by sequentially growing an AlN buffer layer, an n-GaN layer, an active region layer, a p-AlGaN electron blocking layer and a p-GaN layer on the substrate through a metal organic chemical vapor deposition technique.
3. The method according to claim 1 or 2, characterized in that: The substrate is a patterned sapphire substrate; Optionally, the patterned sapphire substrate is a sapphire substrate having a periodic conical sapphire or SiO2 array on the surface; Optionally, the height of the cavity microstructure is 3-5 μm.
4. The method according to any one of claims 1 to 3, characterized in that: The deposition of a SiO2 protective layer on the surface of the p-GaN layer is performed by plasma enhanced chemical vapor deposition technology.
5. The method according to any one of claims 1 to 4, characterized in that: The wavelength of the nanosecond pulse laser is 355nm; Optionally, the repetition frequency of the nanosecond pulse laser is 20-100 kHz; Optionally, the output power of the nanosecond pulse laser is 0.1-2W.
6. The method according to any one of claims 1 to 5, characterized in that: The width of the groove is 2-6 μm.
7. The method according to any one of claims 1 to 6, characterized in that: The solution used for the thermochemical corrosion is a mixed solution of H3PO4 and H2SO4; Optionally, the ratio of the mixed solution of H3PO4 and H2SO4 is 3 to 1; Optionally, the thermochemical etching temperature is 200-300°C; Optionally, the thermochemical etching time is 1 to 30 minutes; Optionally, the thermochemical etching time is 5 minutes.
8. The method according to any one of claims 1 to 7, characterized in that: The SiO2 protective layer in the removal step 2) is removed by wet etching technology; Optionally, etching the ITO layer to form a patterned ITO layer further includes etching the epitaxial layer by photolithography and dry etching techniques until the p-GaN layer is exposed.
9. The method according to any one of claims 1 to 8, characterized in that: Before the p-electrode and the n-electrode are evaporated on the SiO2 passivation layer, the method further includes etching the p-through hole and the n-through hole on the SiO2 passivation layer respectively by using photolithography and dry etching technology.
10. A Micro-LED chip, characterized in that: The Micro-LED chip is prepared by the method according to any one of claims 1 to 9.