Positive electrode lithium supplement agent and preparation method thereof, positive electrode slurry and lithium ion battery
Through the composite structure of nano lithium carbonate and nano conductive carbon black as the positive electrode lithium supplement agent, the problem of irreversible capacity loss in lithium-ion batteries is solved, the initial charging capacity and stability of the battery are improved, and it is suitable for the application of lithium-ion batteries.
Patent Information
- Application Number
- CN202411386289.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
During the first charging and discharging process of existing lithium-ion batteries, irreversible capacity loss caused by the passivation layer formed by the electrolyte and electrode reaction, which affects the initial Coulomb efficiency and energy density of the battery. The existing positive lithium supplement is unstable or provided in the air. The number of activity is limited.
The composite structure of nano-conductive carbonate particles and nano-conductive carbon black is used as the positive electrode lithium supplement agent. The core-shell structure of nano-conductive carbon black is formed by ball milling to completely coat nano-conductive carbon black, which improves reaction activity and reduces the decomposition potential.
The initial charging capacity has been increased to 645.2mAh/g, the decomposition potential has been reduced to 3.8V, and it is stable in the air, adapted to the battery system, and has good application prospects.
Smart Images

Figure BDA0005071047150000141 
Figure BDA0005071047150000151 
Figure BDA0005071047150000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials and relates to a positive electrode lithium supplement and a preparation method thereof, a positive electrode slurry and a lithium ion battery. Background Art
[0002] In recent years, due to the rapid development of electronic products and new energy vehicles, higher requirements have been placed on the energy density and cycle life of lithium-ion batteries. However, during the first charge and discharge process of lithium-ion batteries, the electrolyte and the electrode react at the solid-liquid interface to form a passivation layer covering the electrode surface, namely the solid electrolyte interface film (SEI). The active lithium ions released from the cathode are one of the main components of the SEI film, and its irreversible capacity loss can reach 10%, resulting in a decrease in the initial coulomb efficiency of the battery and a decrease in energy density. In order to solve this problem, people have studied pre-lithiation technology.
[0003] Pre-lithiation technology refers to adding lithium into the battery before the battery is working to replenish lithium ions in order to offset the irreversible lithium loss caused by the formation of the SEI film. It is usually divided into two categories: positive electrode lithium replenishment and negative electrode lithium replenishment.
[0004] Negative electrode lithium replenishment is mainly achieved through lithium powder, lithium foil and lithium-containing reagents. Due to the high reactivity of metallic lithium and strict environmental requirements, it is difficult to use it in large quantities in actual production. In contrast, positive electrode lithium replenishment is more promising because it allows lithium replenishment materials to be added directly to the slurry, which is compatible with the current manufacturing process of lithium-ion batteries. Therefore, a large number of positive electrode lithium replenishment additives have been studied.
[0005] From the perspective of practical application, an ideal lithium ion supplement should meet four basic requirements: suitable lithium potential, sufficient stability, high irreversible capacity and compatibility with the manufacturing process of existing lithium ion batteries. Small molecule lithium salts Li2O, Li2O2, Li3N and Li2S with high irreversible capacity are widely used as positive electrode lithium supplements, but they have some disadvantages, such as instability in the atmosphere, and a large amount of gas and residue will be generated after the release of lithium ions to damage the performance of lithium ion batteries; the mixture of lithium-containing small molecules and transition metals (such as Co, CoO) can also achieve the effect of lithium supplementation, but the inactive Co3O4 residue will damage the battery's cycle performance; lithium salts containing metal oxides Li6CoO4, Li5FeO4, Li2NiO2 are also unstable in the air and provide a limited number of active lithium; organic lithium salts (such as Li2C2O4) can also be used as lithium supplements. Although they are stable in the air and have good compatibility with the battery system, their irreversible capacity is relatively low, and more volume is required to fill the lithium supplement, which has a certain impact on the battery energy density. Therefore, further research is needed on positive electrode lithium supplement additives.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] In view of the deficiencies and defects in the prior art, the present invention aims to provide a positive electrode lithium supplement and a preparation method thereof, a positive electrode slurry and a lithium ion battery.
[0008] In order to achieve the above purpose, the following technical solutions are adopted:
[0009] The first object of the present invention is to provide a positive electrode lithium supplement, comprising nano lithium carbonate particles and nano conductive carbon black coated on the surface of the nano lithium carbonate particles.
[0010] Furthermore, based on the above technical solution of the present invention, the nano conductive carbon black includes at least one of Ketjen black, Super-P or acetylene black.
[0011] Further, on the basis of the above technical solution of the present invention, the nano lithium carbonate particles are spherical nano particles with a particle size of 50-150nm;
[0012] And / or, the nano conductive carbon black is spherical nanoparticles with a particle size of 20-50 nm.
[0013] Furthermore, based on the above technical solution of the present invention, the mass ratio of the nano lithium carbonate particles to the nano conductive carbon black is (4-1):1.
[0014] The second object of the present invention is to provide a method for preparing a positive electrode lithium supplement, comprising the following steps:
[0015] The lithium carbonate and the conductive carbon black are mixed and then ball-milled to obtain a positive electrode lithium supplement having a composite structure of nano-conductive carbon black coated with nano-lithium carbonate.
[0016] Furthermore, based on the above technical solution of the present invention, the mass ratio of the lithium carbonate to the conductive carbon black is (4-1):1.
[0017] Further, based on the above technical solution of the present invention, the ball milling speed is 500-1500rpm;
[0018] And / or, the ball milling is wet ball milling, and the solvent used in the wet ball milling includes ethanol.
[0019] The third object of the present invention is to provide a positive electrode slurry, comprising an active material, a conductive agent, a binder and a positive electrode lithium supplement;
[0020] Wherein, the positive electrode lithium replenisher is the positive electrode lithium replenisher provided by the first purpose of the present invention or the positive electrode lithium replenisher prepared by the preparation method provided by the second purpose of the present invention.
[0021] Further, on the basis of the above technical solution of the present invention, the active material includes a nickel-cobalt-lithium manganese oxide ternary material;
[0022] and / or, the conductive agent comprises conductive carbon black;
[0023] and / or, the binder comprises polyvinylidene fluoride;
[0024] And / or, the mass ratio of the active material, the conductive agent and the binder is (80-98): (10-1): (10-1);
[0025] And / or, the mass ratio of the active material to the positive electrode lithium supplement agent is (90-98): (10-2).
[0026] The fourth object of the present invention is to provide a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises the positive electrode lithium supplement provided by the first object of the present invention or is made of the positive electrode slurry provided by the third object of the present invention.
[0027] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:
[0028] (1) The present invention provides a positive electrode lithium replenisher, which is formed by compounding nano lithium carbonate and nano conductive carbon black to form a nano composite structure in which nano conductive carbon black completely covers nano lithium carbonate. Compared with conventional micron-sized lithium carbonate, the reaction activity of the nano composite structure is greatly improved, the decomposition potential can be reduced to 3.8V, and the initial charging capacity is increased to 645.2mAh / g. It can be used as a positive electrode lithium replenisher and has a good lithium replenishment effect. In addition, the positive electrode lithium replenisher is stable in the air, compatible with the battery system, and has a high lithium replenishment capacity, and has a good application prospect.
[0029] (2) The present invention provides a method for preparing the above-mentioned positive electrode lithium supplement agent. The raw materials used in the preparation method are widely available and have good stability. At the same time, the ball milling process used is simple, convenient and easy to operate, has significant practicality, and is conducive to industrial promotion.
[0030] (3) The present invention provides a positive electrode slurry or a lithium ion battery, comprising the above-mentioned positive electrode lithium replenisher. In view of the good lithium replenishing effect of the positive electrode lithium replenisher, the electrochemical performance of the positive electrode slurry or the lithium ion battery comprising the positive electrode slurry or the lithium ion battery is further improved. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0032] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0033] According to a first aspect of the present invention, a positive electrode lithium supplement is provided, comprising nano lithium carbonate particles and nano conductive carbon black coated on the surface of the nano lithium carbonate particles.
[0034] Specifically, the lithium source of the positive electrode lithium supplement of the present invention mainly comes from lithium carbonate (Li2CO3). Lithium carbonate has a high theoretical gram capacity (~724mAh / g), is compatible with the battery system and can exist stably in the atmosphere, and is considered to be one of the most promising positive electrode lithium supplements. However, the commonly used commercial lithium carbonate with a size of micrometers also has some problems, such as low electronic conductivity and a decomposition voltage as high as 4.6V. Therefore, it is necessary to perform some treatment on the commercial lithium carbonate with a size of micrometers to improve its electronic conductivity and reduce the decomposition potential.
[0035] The inventor of the present invention has found through a large number of experimental studies that, unlike the commonly used commercial lithium carbonate at the micron level, the lithium carbonate at the nanometer level (nano lithium carbonate) has a greatly increased surface area, thereby enhancing the reactivity of lithium carbonate, and the decomposition potential of nano lithium carbonate can be reduced to 4.3V, and the initial charging capacity is increased from 25.4mAh / g of micron lithium carbonate to 189.9mAh / g. Although the reactivity has been improved, the decomposition potential of 4.3V is still high relative to lithium-ion batteries, and the charging capacity is only about 26% of the theoretical capacity, and it is still necessary to further reduce the decomposition potential and increase the charging capacity.
[0036] After further in-depth research, it was found that when the surface of nano lithium carbonate is coated with nano conductive carbon black to form a nano composite structure in which nano conductive carbon black completely covers nano lithium carbonate (the formed nano composite structure is similar to a core-shell structure, in which nano lithium carbonate particles are equivalent to the core, and nano conductive carbon black coated on the surface of nano lithium carbonate particles is equivalent to the shell), the reaction activity is further greatly improved through the composite of nano lithium carbonate and nano conductive carbon black, the decomposition potential can be reduced to 3.8V, and the initial charge capacity is increased to 645.2mAh / g, which can be used as a positive electrode lithium supplement. Moreover, the positive electrode lithium supplement is stable in the air, compatible with the battery system, and has a high lithium supplement amount, and has good application prospects.
[0037] It should be noted that the decomposition potential and initial charge capacity of the above-mentioned micron-sized lithium carbonate, nano-lithium carbonate and the composite structure formed by nano-lithium carbonate and nano-conductive carbon black can be obtained by using them as positive electrode materials to make button batteries and performing charge and discharge tests on the button batteries (charge and discharge curves and dQ / dV curves can be drawn).
[0038] There is no specific limitation on the specific type of nano-conductive carbon black, and Ketjen black (KB), Super-P, and acetylene black commonly used in the art may be selected.
[0039] As an optional embodiment of the technical solution of the present invention, the nano lithium carbonate particles are spherical nano particles with a particle size of 50-150nm. The typical but non-limiting particle size of the nano lithium carbonate particles is 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm or 150nm, etc. and the numerical range between any two points.
[0040] As an optional implementation of the technical solution of the present invention, the nano conductive carbon black is a spherical nanoparticle with a particle size of 20-50nm. The typical but non-limiting particle size of the nano conductive carbon black is 20nm, 25nm, 30nm, 35nm, 40nm, 45nm or 50nm, etc., and the numerical range between any two points.
[0041] Further optimization of the specific shape and size of nano lithium carbonate particles and nano conductive carbon black is conducive to the close embedding (or coating) of nano conductive carbon black particles on the surface of nano lithium carbonate particles, forming a nano composite structure in which the conductive agent completely coats the nano lithium carbonate, greatly improving its reaction activity.
[0042] The degree of coating of nano-conductive carbon black on the surface of nano-lithium carbonate particles is related to the relative amounts of the two.
[0043] As an optional implementation of the technical solution of the present invention, the mass ratio of nano lithium carbonate particles to nano conductive carbon black is (4-1): 1. Typical but non-limiting mass ratios are 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1 or 1:1, etc.
[0044] When the mass ratio of nano lithium carbonate particles and nano conductive carbon black is within the numerical range specified in the present invention, a relative balance between the lithium supplement effect and the comprehensive performance of the battery can be achieved. Nano conductive carbon black has a large specific surface area and is an inactive substance. Adding too much nano conductive carbon black will affect the energy density and self-discharge performance of the battery to a certain extent; however, if the amount added is too little, some nano lithium carbonate particles cannot be coated with the conductive agent, which will affect the lithium supplement effect of nano lithium carbonate.
[0045] According to a second aspect of the present invention, there is also provided a method for preparing a positive electrode lithium supplement, comprising the following steps:
[0046] The lithium carbonate and the conductive carbon black are mixed and then ball-milled to obtain a positive electrode lithium supplement having a composite structure of nano-conductive carbon black coated with nano-lithium carbonate.
[0047] Specifically, lithium carbonate may be lithium carbonate commonly used in the market, such as commercial lithium carbonate with a size of micrometer level. Conductive carbon black may be common types, such as Ketjen black.
[0048] Ketjen black is mainly a fiber branch structure formed by primary particles agglomerated together. The agglomerated primary particles can be dispersed by ball milling. The size of the dispersed primary particles can remain unchanged, and the primary particles can also be crushed into small-sized spherical nanoparticles. Ketjen black has a smaller particle size and a larger specific surface area. It has a better dispersion effect on lithium carbonate particles during ball milling, making the size of lithium carbonate more uniform and the sphere more regular, and finally obtaining a nano-composite structure in which nano-conductive carbon black particles are tightly embedded (completely coated) on the surface of nano-lithium carbonate spherical particles.
[0049] The raw materials used in the preparation method of the present invention are widely available and have good stability. At the same time, the ball milling process used is simple, convenient and easy to operate, has significant practicality, and is conducive to industrial promotion.
[0050] As an optional implementation of the technical solution of the present invention, the mass ratio of lithium carbonate to conductive carbon black is (4-1): 1. Typical but non-limiting mass ratios are 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1 or 1:1, etc.
[0051] As an optional embodiment of the technical solution of the present invention, the speed of the ball mill is 500-1500 rpm. Typical but non-limiting ball mill speeds are 500 rpm, 600 rpm, 800 rpm, 900 rpm, 1000 rpm, 1200 rpm, 1400 rpm or 1500 rpm, and the like, and the numerical range between any two points.
[0052] As an optional implementation of the technical solution of the present invention, the ball milling is wet ball milling, and the solvent used in the wet ball milling includes ethanol.
[0053] By further limiting the process parameters of the ball milling process, lithium carbonate and conductive carbon black can be completely coated at the nanoscale, thereby improving the reaction activity of the lithium supplement.
[0054] According to a third aspect of the present invention, there is also provided a positive electrode slurry, comprising an active material, a conductive agent, a binder, a positive electrode lithium supplement and a solvent;
[0055] The positive electrode lithium replenisher is the positive electrode lithium replenisher provided by the first aspect of the present invention or the positive electrode lithium replenisher prepared by the preparation method of the second aspect of the present invention.
[0056] As an optional implementation of the technical solution of the present invention, the active material includes nickel cobalt manganese oxide (NCM) ternary material, preferably at least one of NCM111, NCM523, NCM613 or NCM811.
[0057] As an optional implementation of the technical solution of the present invention, the conductive agent includes conductive carbon black, such as Super P, Ketjen black, acetylene black, etc.
[0058] As an optional implementation of the technical solution of the present invention, the binder includes polyvinylidene fluoride, and the model is, for example, HSV900, solef 5130, etc.
[0059] As an optional implementation of the technical solution of the present invention, the solvent includes N-methylpyrrolidone (NMP).
[0060] As an optional implementation of the technical solution of the present invention, the mass ratio of the active material, the conductive agent and the binder is (80-98): (10-1): (10-1). Typical but non-limiting mass ratios of the active material, the conductive agent and the binder are 80:10:10, 86:7:7, 90:5:5, 95:2.5:2.5, 96:2:2, 96.5:1.5:2, 97:1.5:1.5, 98:1:1, etc.
[0061] As an optional implementation of the technical solution of the present invention, the mass ratio of the active material to the positive electrode lithium replenisher is (90-98): (10-2).
[0062] The positive electrode lithium replenisher and the active material can achieve a relative balance between the lithium replenishment effect and the performance of the battery cell within the numerical range specified in the present invention. If the amount of the positive electrode lithium replenisher is too much, the excessive lithium ions cannot be embedded in the negative electrode and are deposited on the surface in the form of lithium dendrites, which has a certain degree of impact on the safety and electrical performance of the battery. If the amount of the positive electrode lithium replenisher is too little, the lithium replenishment effect on the battery is limited, and the performance of the lithium replenisher cannot be fully exerted. Therefore, the typical but non-restrictive mass ratio of the active material and the positive electrode lithium replenisher is 90:10, 90:8, 90:5, 90:2, 92:10, 92:8, 92:5, 92:2, 95:10, 95:8, 95:5, 95:2, 98:10, 98:8, 98:5 or 98:2, etc.
[0063] According to a fourth aspect of the present invention, a lithium ion battery is further provided, wherein the positive electrode of the lithium ion battery comprises the positive electrode lithium supplement provided by the first aspect of the present invention or is made of the positive electrode slurry provided by the third aspect of the present invention.
[0064] In view of the advantages of the positive electrode lithium supplement or positive electrode slurry provided by the present invention, the lithium ion battery prepared therefrom has good electrochemical properties.
[0065] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0066] Example 1
[0067] This embodiment provides a positive electrode lithium supplement, comprising nano lithium carbonate particles and nano conductive carbon black coated on the surface of the nano lithium carbonate particles;
[0068] Among them, the nano lithium carbonate particles are spherical nano particles with an average particle size of 100nm; the nano conductive carbon black is spherical nano Kejen black particles with an average particle size of 30nm; the mass ratio of the nano lithium carbonate particles to the nano conductive carbon black is 2:1.
[0069] The preparation method of the positive electrode lithium supplement agent in this embodiment comprises the following steps:
[0070] Commercial lithium carbonate (30 μm in length, 5 μm in diameter, and a hexagonal columnar structure) and Ketjen black (having primary particles (average particle size of 30 nm) aggregated together to form a fibrous branching structure) were mixed in a mass ratio of 2:1 and then ball-milled. The ball-milling speed was 500 rpm, the ball-milling time was 12 h, the ball-milling method was wet ball-milling, and the ball-milling dispersion solvent was ethanol. After the ball-milling was completed, a high-speed desktop centrifuge was used to separate and remove the ethanol solvent at a speed of 5000 rpm. The obtained powder was dried in an oven at 80°C for 12 h to obtain a positive electrode lithium supplement having a composite structure of nano-conductive carbon black coated with nano-lithium carbonate.
[0071] Example 2
[0072] This embodiment provides a positive electrode lithium supplement agent, except that the mass ratio of nano lithium carbonate particles and nano conductive carbon black is adjusted from 2:1 to 1:1, the remaining raw material composition is the same as that of Example 1.
[0073] In the preparation method of the positive electrode lithium supplement agent of this embodiment, except that the mass ratio of commercial lithium carbonate and conductive carbon black is adjusted from 2:1 to 1:1, the other methods and process parameters are the same as those of Example 1.
[0074] Example 3
[0075] This embodiment provides a positive electrode lithium supplement, except that the mass ratio of nano lithium carbonate particles and nano conductive carbon black is adjusted from 2:1 to 4:1, the remaining raw material composition is the same as that of Example 1.
[0076] In the preparation method of the positive electrode lithium supplement agent of this embodiment, except that the mass ratio of commercial lithium carbonate and conductive carbon black is adjusted from 2:1 to 4:1, the other methods and process parameters are the same as those of Example 1.
[0077] Example 4
[0078] This embodiment provides a positive electrode lithium supplement, except that the average particle size of nano lithium carbonate particles is adjusted from 100nm to 200nm; the average particle size of nano conductive carbon black (nano Ketjen black) is adjusted from 30nm to 60nm, and the remaining raw material composition is the same as that of Example 1.
[0079] In the preparation method of the positive electrode lithium supplement agent of this embodiment, the Ketjen black used has a fiber branch structure formed by primary particles (average particle size of 60nm) aggregated together, the ball milling time is reduced from 12h to 6h, and the other methods and process parameters are the same as those in Example 1.
[0080] Example 5
[0081] This embodiment provides a positive electrode lithium supplement agent, except that the nano conductive carbon black coated on the surface of the nano lithium carbonate particles is Super P (whose average particle size is 30nm), the rest of the raw material composition is the same as that of Example 1.
[0082] Example 6
[0083] This embodiment provides a positive electrode slurry, comprising an active material NCM523, a conductive agent SP, a binder PVDF-5130, a positive electrode lithium supplement provided in Example 1, and a solvent NMP;
[0084] Among them, the mass ratio of active material NCM523, conductive agent SP, and binder PVDF is 97:1:2, and the mass ratio of active material NCM523 to positive electrode lithium supplement agent is 95:5.
[0085] The method for preparing the positive electrode slurry in this embodiment comprises the following steps:
[0086] (a) mixing the binder PVDF-5130 powder and the solvent NMP uniformly to obtain a glue solution with a solid content of 5±1%;
[0087] (b) adding a conductive agent SP (the mass ratio of the conductive agent SP to the binder PVDF-5130 is 1:2) into the glue solution, stirring at a speed of 1800 RPM for 1 h to obtain a conductive slurry;
[0088] (c) The active material NCM523 and the positive electrode lithium replenisher (the mass ratio of the active material NCM523 to the positive electrode lithium replenisher is 95:5) are added to the conductive slurry at a mass ratio of NMC523:SP:PVDF=97:1:2, and stirred at a speed of 1800RPM for 3 hours to finally obtain a positive electrode slurry with a solid content of 50±2%.
[0089] Example 7
[0090] This embodiment provides a positive electrode slurry. Except for adjusting the mass ratio of the active material NCM523 to the positive electrode lithium supplement agent from 95:5 to 90:10, the other raw materials and composition are the same as those in Example 6.
[0091] The method for preparing the positive electrode slurry of this embodiment is the same as that of Example 6, except that the mass ratio of the active material NCM523 to the positive electrode lithium supplement in step (c) is adjusted from 95:5 to 90:10. The remaining steps and process parameters are the same as those of Example 6.
[0092] Example 8
[0093] This embodiment provides a positive electrode slurry. Except for adjusting the mass ratio of the active material NCM523 to the positive electrode lithium supplement agent from 95:5 to 98:2, the other raw materials and composition are the same as those in Example 6.
[0094] The method for preparing the positive electrode slurry of this embodiment is the same as that of Example 6, except that the mass ratio of the active material NCM523 to the positive electrode lithium supplement in step (c) is adjusted from 95:5 to 98:2. The remaining steps and process parameters are the same as those of Example 6.
[0095] Example 9
[0096] This embodiment provides a positive electrode slurry. Except that the positive electrode lithium replenisher is the positive electrode lithium replenisher provided in Embodiment 2, the other raw materials and composition are the same as those in Embodiment 6.
[0097] The method for preparing the positive electrode slurry of this embodiment is the same as that of Embodiment 6 except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Embodiment 2. The remaining steps and process parameters are the same as those of Embodiment 6.
[0098] Example 10
[0099] This embodiment provides a positive electrode slurry. Except that the positive electrode lithium replenisher is the positive electrode lithium replenisher provided in Embodiment 3, the other raw materials and composition are the same as those in Embodiment 6.
[0100] The method for preparing the positive electrode slurry of this embodiment is the same as that of Embodiment 6 except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Embodiment 3. The remaining steps and process parameters are the same as those of Embodiment 6.
[0101] Embodiment 11
[0102] This embodiment provides a positive electrode slurry. Except that the positive electrode lithium replenisher is the positive electrode lithium replenisher provided in Embodiment 4, the other raw materials and composition are the same as those in Embodiment 6.
[0103] The method for preparing the positive electrode slurry of this embodiment is the same as that of Embodiment 6 except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Embodiment 4. The remaining steps and process parameters are the same as those of Embodiment 6.
[0104] Example 12
[0105] This embodiment provides a positive electrode slurry. Except that the positive electrode lithium replenisher is the positive electrode lithium replenisher provided in Embodiment 5, the other raw materials and composition are the same as those in Embodiment 6.
[0106] The method for preparing the positive electrode slurry of this embodiment is the same as that of Embodiment 6 except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Embodiment 5. The remaining steps and process parameters are the same as those of Embodiment 6.
[0107] Comparative Example 1
[0108] This comparative example provides a positive electrode lithium supplement agent, except that the nano lithium carbonate particles are not coated with nano Ketjen black, that is, the positive electrode lithium supplement agent is only nano lithium carbonate, and the other raw materials and dosages are the same as those in Example 1;
[0109] The preparation method of the positive electrode lithium supplement agent of this comparative example comprises the following steps:
[0110] Commercial lithium carbonate (30 μm in length, 5 μm in diameter, and a hexagonal columnar structure) was ball-milled at a ball-milling speed of 500 rpm for 12 h in a dry ball-milling method to obtain a lithium carbonate positive electrode lithium supplement having a nanostructure.
[0111] Comparative Example 2
[0112] This comparative example provides a positive electrode lithium supplement, except that the nano lithium carbonate particles are replaced by nano lithium oxide particles (average particle size of 100 nm), the other raw materials and dosages are the same as those in Example 1;
[0113] In the preparation method of the positive electrode lithium supplement of this comparative example, commercial lithium carbonate is replaced by lithium oxide (particle size of 1-50 μm, a mixture of particles in various forms), and the remaining steps and process parameters are the same as those in Example 1.
[0114] Comparative Example 3
[0115] This comparative example provides a positive electrode slurry. Except that the positive electrode lithium replenisher in Example 6 is replaced by the positive electrode lithium replenisher provided in Comparative Example 1, the other raw materials and amounts are the same as those in Example 6.
[0116] The preparation method of the positive electrode slurry of this comparative example is the same as that of Example 6, except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Comparative Example 1. The remaining steps and process parameters are the same as those of Example 6.
[0117] Comparative Example 4
[0118] This comparative example provides a positive electrode slurry. Except that the positive electrode lithium replenisher in Example 6 is replaced by the positive electrode lithium replenisher provided in Comparative Example 2, the other raw materials and amounts are the same as those in Example 6.
[0119] The preparation method of the positive electrode slurry of this comparative example is the same as that of Example 6, except that the positive electrode lithium replenisher in step (c) is adjusted to the positive electrode lithium replenisher provided in Comparative Example 2. The remaining steps and process parameters are the same as those of Example 6.
[0120] Comparative Example 5
[0121] This comparative example provides a positive electrode slurry. Except that no positive electrode lithium supplement agent is added in Example 6, the other raw materials and amounts are the same as those in Example 6.
[0122] The preparation method of the positive electrode slurry in this comparative example is the same as that of Example 6, except that no positive electrode lithium supplement agent is added in step (c).
[0123] In order to compare the technical effects of the above embodiments and comparative examples, the following experimental examples are specially designed.
[0124] Experimental Example 1
[0125] The positive electrode slurries provided in Examples 6-12 and Comparative Examples 3-5 were made into positive electrode sheets, which were then assembled into lithium-ion batteries. The specific manufacturing method is as follows:
[0126] 1. Preparation of positive electrode sheet:
[0127] The above positive electrode slurries were uniformly coated on a 13 μm carbon-coated aluminum foil using a transfer coater to obtain a surface density of 330 ± 3 g / m 2 The positive electrode;
[0128] 2. Preparation of negative electrode sheet:
[0129] (a) dissolving CMC-2200 powder in deionized water and stirring to mix well to obtain a glue solution with a solid content of 1.5±0.5%;
[0130] (b) dry mixing the negative electrode main material graphite and SP at a rotation speed of 1500 RPM for 0.5 h to obtain a mixture;
[0131] (c) adding an appropriate amount of deionized water and a certain amount of SBR and CMC glue (wherein the negative electrode main material: SP: SBR: CMC = 96: 1: 1.5: 1.5, by mass ratio) to the above mixture, and stirring at a high speed of 2500 RPM to finally obtain a negative electrode slurry with a solid content of 50 ± 2%;
[0132] (d) The above slurry was evenly coated on a 6 μm copper foil using a transfer coater to obtain a surface density of 200 ± 3 g / m 2 The negative electrode;
[0133] 3. Preparation of lithium-ion batteries:
[0134] The positive electrode sheets and negative electrode sheets are rolled, die-cut and slit to form a core package, and then the electrolyte is injected to assemble into a battery cell, which is then baked, injected with liquid, left standing at high temperature, formed and divided into volumes to obtain a lithium-ion battery.
[0135] The lithium-ion batteries made of the positive electrode slurries of Examples 6-12 and Comparative Examples 3-6 were subjected to charge and discharge tests, DCR tests, and 25°C 1C / 1C cycles.
[0136] Initial efficiency and discharge capacity test: At 25°C, charge the lithium-ion battery at a constant current of 1 / 3C to 4.25V, then charge at a constant voltage of 4.2V until the current is less than 0.05C, record the initial charge capacity, and then discharge at a constant current of 1 / 3C to 2.8V, record the initial discharge capacity;
[0137] First efficiency = first discharge capacity / first charge capacity*100%.
[0138] DCR test process steps: the initial test temperature is 25±2℃, each group of cells is charged to 3.65V at 1C, then charged to 0.05C at a constant voltage, left for 10min, discharged to 30min at 1C, left for 10min, the voltage after leaving is recorded as V1, discharged for 10s at 2C current (recorded as I), the voltage after discharge is recorded as V2, then DCR = (V1-V2) / I.
[0139] 25℃1C / 1C cycle test process: The initial test temperature is 25±2℃, and each group of batteries is charged to 3.65V at 1C, then charged to 0.05C at a constant voltage, left for 10 minutes, and then discharged to 2.5V at 1C, left for 10 minutes. The above steps are repeated until the capacity drops to 80% of the initial capacity.
[0140] The specific results are shown in Table 1
[0141] Table 1
[0142]
[0143]
[0144] It can be seen from the data in Table 1 that, compared with the lithium-ion battery of Comparative Example 5 in which no lithium supplement is added, each embodiment in which the lithium supplement is added can significantly improve the first efficiency and discharge capacity of the battery.
[0145] Comparing Example 6 with Example 7, the capacity and the first effect are not much different, but the DC internal resistance of Example 7 is significantly higher than that of Example 6, indicating that the amount of lithium supplement in Example 6 is sufficient to offset the lithium ion loss when the SEI film is formed, while in Example 7, a slightly larger amount of lithium supplement is added, and the number of lithium ions in the battery is relatively large, which may precipitate in the negative electrode in the form of lithium dendrites, increasing the DC internal resistance of the battery. Comparing Example 6 with Example 8, the amount of lithium supplement added in Example 8 is slightly less, and the lithium supplement depth may be insufficient to offset the lithium ion loss of the SEI film, resulting in a slightly lower first effect and discharge capacity. But overall, compared with Comparative Example 5, Examples 7 and 8 have a certain improvement effect on the first effect and discharge capacity of lithium-ion batteries.
[0146] Example 6, Example 9 and Example 10 compare the effect of the mass ratio of lithium carbonate and Ketjen black on battery performance. In Example 9, when the relative amount of the conductive agent increased, the improvement of the first efficiency and capacity of the battery was limited, and the DC internal resistance decreased; in Example 10, the relative amount of the conductive agent decreased, which may cause some nano lithium carbonate not to be coated with the conductive agent, and the first efficiency and capacity of the battery decreased; Example 6 and Example 11 compare the effect of the particle size of lithium carbonate and Ketjen black on battery performance. As the particle size increases, the reactive area decreases, and the first efficiency and capacity of the battery decrease. Example 6 and Example 12 compare the effect of the type of conductive agent on battery performance. Compared with SP, nano Ketjen black has a larger specific surface area and more reactive sites, so the nanometer battery with nano Ketjen black has a higher first efficiency and capacity than the battery with SP.
[0147] In Comparative Example 3, the nano lithium carbonate is not coated with a conductive agent, and the nano lithium carbonate has basically no reaction activity, which is close to the effect of Comparative Example 5 without adding a lithium supplement. In Comparative Example 4, lithium oxide is used as a lithium source in the positive electrode lithium supplement, but because lithium oxide is unstable, metal dissolution is prone to occur under high pressure, which has a certain negative impact on the initial efficiency and capacity of the battery.
[0148] Table 2 shows the cycle performance data of lithium-ion batteries made from the positive electrode slurries of Examples 6-12 and Comparative Examples 3-6, as shown in Table 2.
[0149] Table 2
[0150]
[0151] It can be seen from the cycle data in Table 2 that, compared with the lithium ion battery of comparative example 5 without adding the lithium replenisher, the capacity retention rate of the lithium ion battery with the positive electrode lithium replenisher added in each embodiment of the present invention is higher than the capacity retention rate of the lithium ion battery of comparative example 5 without adding the lithium replenisher.
[0152] Comparing Example 6 with Example 7, the amount of lithium supplement added in Example 7 is slightly more, which may cause excessive lithium supplementation, forming lithium dendrites at the negative electrode, which has a certain negative impact on the cycle performance and also affects the safety performance; comparing Example 6 with Example 8, the amount of lithium supplement added in Example 8 is slightly less, which may not replenish the lithium enough, and the ability to improve the cycle performance is limited. However, overall, compared with Comparative Example 5 in which no lithium supplement is added, adding positive electrode lithium supplement has a significant effect on improving the cycle performance of lithium-ion batteries.
[0153] Example 6, Example 9 and Example 10 compare the effect of the mass ratio of nano lithium carbonate and nano Ketjen black on the battery cycle performance. Compared with Example 6, when the amount of conductive agent in Example 9 increases, the side reaction active sites increase, and the cycle performance decreases slightly; when the amount of conductive agent in Example 10 decreases, it is possible that part of the nano lithium carbonate is not completely coated by the conductive agent, and the role of the lithium supplement agent cannot be fully exerted, and the cycle performance will also decrease. Example 6 and Example 11 compare the effect of the particle size of nano lithium carbonate and nano Ketjen black on battery performance. When the particle size increases, the reactive area decreases, and the battery cycle will decrease. Example 6 and Example 12 compare the effect of the type of conductive agent on battery performance. Compared with SP, nano Ketjen black has a larger specific surface area and more reactive sites, so the battery using nano Ketjen black has higher cycle performance.
[0154] In Comparative Example 3, the lithium carbonate is not coated with a conductive agent, and the nano lithium carbonate has basically no reaction activity, which is similar to the effect of Comparative Example 5 without adding a lithium supplement. In Comparative Example 4, lithium oxide is used as a lithium source in the positive electrode lithium supplement, but because lithium oxide is unstable, metal dissolution is prone to occur under high pressure, which has a certain impact on the battery cycle performance.
[0155] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A positive electrode lithium supplement, characterized in that: The invention comprises nano lithium carbonate particles and nano conductive carbon black coated on the surface of the nano lithium carbonate particles.
2. The positive electrode lithium supplement according to claim 1, characterized in that: The nano conductive carbon black includes at least one of Ketjen black, Super-P or acetylene black.
3. The positive electrode lithium supplement according to claim 1, characterized in that: The nano lithium carbonate particles are spherical nano particles with a particle size of 50-150nm; And / or, the nano conductive carbon black is spherical nanoparticles with a particle size of 20-50 nm.
4. The positive electrode lithium supplement according to any one of claims 1 to 3, characterized in that: The mass ratio of the nano lithium carbonate particles to the nano conductive carbon black is (4-1):
1.
5. The method for preparing the positive electrode lithium supplement according to any one of claims 1 to 4, characterized in that: The following steps are involved: The lithium carbonate and the conductive carbon black are mixed and then ball-milled to obtain a positive electrode lithium supplement having a composite structure of nano-conductive carbon black coated with nano-lithium carbonate.
6. The method for preparing a positive electrode lithium supplement according to claim 5, characterized in that: The mass ratio of the lithium carbonate to the conductive carbon black is (4-1):
1.
7. The method for preparing a positive electrode lithium supplement according to claim 5, characterized in that: The ball milling speed is 500-1500rpm; And / or, the ball milling is wet ball milling, and the solvent used in the wet ball milling includes ethanol.
8. A positive electrode slurry, characterized in that: It contains active material, conductive agent, binder and positive electrode lithium supplement agent; Wherein, the positive electrode lithium replenisher is the positive electrode lithium replenisher according to any one of claims 1 to 4 or the positive electrode lithium replenisher prepared by the preparation method according to any one of claims 5 to 7.
9. The positive electrode slurry according to claim 8, characterized in that: The active material includes a nickel-cobalt-lithium manganese oxide ternary material; and / or, the conductive agent comprises conductive carbon black; and / or, the binder comprises polyvinylidene fluoride; And / or, the mass ratio of the active material, the conductive agent and the binder is (80-98): (10-1): (10-1); And / or, the mass ratio of the active material to the positive electrode lithium supplement agent is (90-98): (10-2).
10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery comprises the positive electrode lithium supplement agent according to any one of claims 1 to 4 or is made of the positive electrode slurry according to claim 8 or 9.
Citation Information
Patent Citations
Method for preparing carbon-coated lithium supplementing material through wet ball milling and application of carbon-coated lithium supplementing material
CN116722142A
Positive electrode lithium supplement additive and preparation method and application thereof
CN118522973A
Cited By
Battery monomer as well as preparation method and application thereof
CN122202541A