Preparation method of oxygen reduction electrocatalyst Mn5.64P3 / CePO4 (at) Cs for zinc air battery

Through the preparation of Mn5.64P3/CePO4@Cs composite material, the coupling effect of rare earth cations and transition metals is used to solve the problems of high cost and poor stability of zinc air battery catalysts, and high-efficiency oxygen reduction activity and stability are achieved. It is suitable for zinc Air batteries and other fuel cells.

CN119050386AInactive Publication Date: 2024-11-29GUANGXI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411150884.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing zinc-air battery catalysts are costly and have poor stability, making it difficult to meet sustainable energy needs, especially the problem of kinetic hysteresis in oxygen reduction reaction (ORR).

Method used

The Mn5.64P3/CePO4@Cs composite material is used as the oxygen reduction electrocatalyst, and synthesized by room temperature stirring and high-temperature annealing process, using the coupling effect of rare earth cations and transition metals to improve electrocatalytic activity and stability.

Benefits of technology

It achieves efficient oxygen reduction activity, good stability and durability, improves kinetic current density, and remains stable in a methanol environment, which is significantly better than traditional catalysts and is suitable for zinc air batteries and other fuel cell applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050386A_ABST
    Figure CN119050386A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an oxygen reduction electrocatalyst Mn5.64P3 / CePO4 (at) Cs for a zinc air battery, and belongs to the technical field of electrocatalytic oxidation reduction.The preparation method comprises the steps that a carbon sphere precursor, cerium salt and manganese salt are mixed in a solvent and stirred at the room temperature, and a Mn-Ce (at) Cs precursor is obtained; and under an inert gas atmosphere, carrying out phosphating treatment on the Mn-Ce (at) Cs precursor to obtain the oxygen reduction electrocatalyst Mn5.64P3 / CePO4 (at) Cs. The oxygen reduction electrocatalyst Mn5.64P3 / CePO4 (at) Cs containing the phosphorus vacancy prepared by the preparation method disclosed by the invention has excellent electrocatalytic oxygen reduction activity and good stability and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrocatalytic oxidation-reduction technology, and in particular relates to an oxygen reduction electrocatalyst Mn for zinc-air batteries. 5.64 Preparation method of P3 / CePO4@Cs. Background Art

[0002] Proton exchange membrane fuel cells (PEMFCs) fueled by renewable hydrogen are widely regarded as one of the most promising solutions due to their competitive advantages such as zero emissions, high efficiency, fast start-up and low initial cost. Zinc-air batteries (ZABs) have attracted great attention due to their high theoretical energy density, cost-effectiveness, environmental sustainability and safety characteristics. PEMFCs convert the chemical energy of hydrogen and oxygen into electrical energy through oxygen reduction reaction (ORR) and hydrogen oxidation reaction (HOR), thereby achieving high conversion efficiency and power density. Among them, ORR is a multi-electron transfer process with kinetic hysteresis, requiring efficient electrocatalytic materials to accelerate the reaction. Although platinum group metal (PGM) catalysts are considered as benchmark catalysts for ORR, their high cost and limited stability seriously hinder their large-scale application. Therefore, exploring low-cost and high-efficiency non-precious metal alternatives is crucial to meet the growing demand for sustainable energy. Summary of the invention

[0003] The present invention aims to provide an oxygen reduction electrocatalyst Mn for zinc-air batteries. 5.64 The preparation method of P3 / CePO4@Cs is used to solve the problems existing in the above-mentioned prior art. The preparation method provided by the present invention is simple, and Mn is synthesized by stirring at room temperature and annealing at high temperature. 5.64 The P3 / CePO4@Cs composite material exhibits excellent electrocatalytic activity, stability and durability. The present invention makes full use of the unsaturated 4f orbital valence electron configuration and abundant coordination sites of rare earth cations, which can effectively participate in the regulation and optimization of electrocatalytic performance, realize the effective coupling of rare earth and transition metal, accelerate the charge transfer rate, provide abundant electrocatalytic active sites, and thus improve the conductivity of the catalyst.

[0004] One of the technical solutions provided by the present invention:

[0005] An oxygen reduction electrocatalyst Mn for zinc-air batteries 5.64 The preparation method of P3 / CePO4@Cs comprises the following steps: mixing a carbon sphere precursor, a cerium salt and a manganese salt in a solvent, stirring at room temperature to obtain a Mn-Ce@Cs precursor; performing a phosphating treatment on the Mn-Ce@Cs precursor under an inert gas atmosphere to obtain the oxygen reduction electrocatalyst Mn 5.64 P3 / CePO4@Cs.

[0006] The carbon sphere precursor, cerium salt and manganese salt are mixed in a solvent, stirred at room temperature, and a Mn-Ce@Cs precursor is obtained through a physical adsorption reaction.

[0007] Preferably, the preparation method of the carbon sphere precursor comprises the following steps: adding potassium hydroxide solution to glucose solution for hydrothermal reaction to obtain the carbon sphere precursor. The volume ratio of the potassium hydroxide solution to the glucose solution is 0.025:40; the concentration of the potassium hydroxide solution is 1 mol / L; the concentration of the glucose solution is 0.5 mol / L; the temperature of the hydrothermal reaction is 180°C and the time is 6 hours.

[0008] Preferably, the usage ratio of the carbon sphere precursor, cerium salt and manganese salt is 100 mg:6 mmol:6 mmol.

[0009] Preferably, the cerium salt is Ce(NO3)2·6H2O, and the manganese salt is MnCl2·4H2O.

[0010] Preferably, the solvent is a mixed solvent of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1:2.

[0011] Preferably, the stirring time is 8 hours.

[0012] Preferably, the phosphating treatment is to mix and grind the Mn-Ce@Cs precursor and red phosphorus, and then keep the mixture at 800-1100°C for 2 hours. More preferably, the phosphating treatment temperature is 1000°C.

[0013] Preferably, the mass ratio of the Mn-Ce@Cs precursor to red phosphorus is 1:2.

[0014] The second technical solution provided by the present invention is:

[0015] An oxygen reduction electrocatalyst Mn for zinc-air batteries 5.64 P3 / CePO4@Cs was prepared by the above preparation method.

[0016] The third technical solution provided by the present invention is:

[0017] An oxygen reduction electrocatalyst Mn for zinc-air battery 5.64 Application of P3 / CePO4@Cs in catalytic oxygen reduction of zinc-air batteries.

[0018] Compared with the prior art, the present invention has the following advantages and technical effects:

[0019] (1) The oxygen reduction electrocatalyst Mn containing phosphorus vacancies prepared by the present invention 5.64P3 / CePO4@Cs has excellent electrocatalytic oxygen reduction activity and good stability and durability. The design of the heterogeneous structure catalyst makes the obtained Mn 5.64 P3 / CePO4@Cs spontaneously forms a built-in electric field, and electrons are transferred from CePO4 to Mn 5.64 P3 can effectively promote the transfer of charges, adjust the electronic structure of active sites, and balance the adsorption strength of reaction intermediates. 5.64 The combination of P3 / CePO4 and carbon support greatly improves the conductivity and catalytic ability, thereby accelerating the electron transfer rate and overall catalytic performance. 5.64 P3 / CePO4@Cs has abundant phosphorus vacancies, which provide sufficient active centers for electrocatalytic reactions and are beneficial to improving electrocatalytic ORR activity;

[0020] (2) The present invention prepares the excellent oxygen reduction electrocatalyst Mn by simple hydrothermal, room temperature adsorption and high temperature phosphating process. 5.64 P3 / CePO4@Cs, the oxygen reduction electrocatalyst has a larger kinetic current density and better stability;

[0021] (3) Through the electrocatalytic oxygen reduction test, the present invention can observe a relatively obvious oxygen reduction peak, indicating that the electrocatalyst prepared by the present invention has good catalytic activity for the oxygen reduction reaction. The electrocatalyst exhibits excellent characteristics in terms of performance such as starting potential, half-wave potential and kinetic current density. In addition, the electrocatalyst of the present invention also demonstrates extremely high methanol resistance and stability, and can maintain a stable current density in a high methanol environment. In the stability test, after 18 hours of timing reaction, it showed a current retention rate of 97%. In contrast, CePO4@Cs and Mn 5.64 The current retention rates of P3@Cs after 9 hours were only 90% and 73%, respectively. These results show that the coupling of rare earth metal phosphate CePO4 greatly improves the Mn 5.64 Therefore, Mn 5.64 P3 / CePO4@Cs has broad prospects in the practical application of methanol fuel cells and metal-air batteries;

[0022] (4) From the test results of ZAB, it can be observed that the aqueous ZAB prepared using the electrocatalyst of the present invention has an excellent peak power density of 168 mW·cm -2 , which is better than the commercial Pt / C catalyst (129 mW·cm -2 ), in addition, the aqueous ZAB also exhibits excellent open circuit voltage, maximum power density, specific capacity and cycle stability, showing good application prospects. These results show that the zinc-air battery prepared by the present invention has significant advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0024] Figure 1 a is the preparation of oxygen reduction electrocatalyst Mn in Example 1 5.64 Basic flow chart of P3 / CePO4@Cs, b is the electrocatalyst Mn prepared in Example 1 5.64 The XRD diagram of P3 / CePO4@Cs, c is the EPR spectrum of the electrocatalysts prepared in Example 1 and Comparative Examples 1-2, d is the N2 adsorption-desorption isotherm and pore size distribution diagram of the electrocatalyst prepared in Example 1, and e is the Mn prepared in Example 1. 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 Comparison of contact angles of P3@Cs and CePO4@Cs prepared in comparative example 2;

[0025] Figure 2 This is a SEM image of the carbon sphere precursor prepared in Example 1;

[0026] Figure 3 Where a is Mn prepared in Example 1 5.64 SEM image of P3 / CePO4@Cs, b is Mn 5.64 TEM images of P3 / CePO4@Cs, c~e are Mn 5.64 High-resolution TEM image of P3 / CePO4@Cs, f is Mn 5.64 HAADF-STEM image and corresponding element mapping of P3 / CePO4@Cs;

[0027] Figure 4 Mn prepared in Example 1 5.64 EDS spectrum of P3 / CePO4@Cs;

[0028] Figure 5a is a UPS diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, b is an energy band structure diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, c is an XPS diagram of the product prepared in Example 1 in the C1s region, d is an XPS diagram of the products prepared in Example 1 and Comparative Example 2 in the Ce 3d region, e is an XPS diagram of the products prepared in Example 1 and Comparative Example 1 in the Mn 2p region, f is an XPS diagram of the products prepared in Example 1 and Comparative Examples 1 to 2 in the P 2p region, and g is an XPS diagram of the products prepared in Example 1 and Comparative Example 2 in the O1s region;

[0029] Figure 6 a is the CV curve of the products prepared in Example 1 and Comparative Examples 1 to 2 in a 0.1 mol / L KOH solution saturated with N2 and O2, b is the LSV polarization curve of the products prepared in Example 1, Comparative Examples 1 to 2 and commercial Pt / C in a 0.1 mol / L KOH solution saturated with O2, c is the Tafel diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, d is the half-wave potential (E) of the products prepared in Example 1 and Comparative Examples 1 to 2 at 0.8 V. 1 / 2 ) and kinetic current density (J k ), e is the double layer capacitance (C dl ) value, f is the oxygen reduction onset potential and half-wave potential (E 1 / 2 ), g is the H2O2 yield (%) and the number of electron transfers (n) of the products prepared in Example 1 and Comparative Examples 1 to 2, h is the methanol tolerance test result of the product prepared in Example 1 and commercial Pt / C, i is the stability test result of the products prepared in Example 1 and Comparative Examples 1 to 2 in an O2-saturated 0.1 mol / L KOH solution (at 1600 rpm);

[0030] Figure 7 a is a schematic diagram of the configuration of the zinc-air battery, b is an open circuit voltage (OCV) diagram of the zinc-air battery, c is a discharge polarization curve and corresponding power density of the zinc-air battery, d is a specific capacity diagram of the zinc-air battery, e is a discharge curve of the zinc-air battery at different current densities, and f is a graph of the Mn in Example 1. 5.64 The LED panel image of ZAB assembled with P3 / CePO4@Cs is lit up. g is the comparison of the power density and specific capacity of the zinc-air battery prepared in Example 5 of the present invention with other recently reported ORR catalysts. h is the power density and specific capacity of the zinc-air battery at 5 mA·cm -2 Electrostatic cycles under (20min per cycle);

[0031] Figure 8 a is Mn prepared in Comparative Example 15.64 a is the XRD pattern of P3@Cs, b is the XRD pattern of CePO4@Cs prepared in Comparative Example 2;

[0032] Fig. 9 a is Mn prepared in Comparative Example 1 5.64 a is the N2 adsorption-desorption isotherm and pore size distribution diagram of P3@Cs, b is the N2 adsorption-desorption isotherm and pore size distribution diagram of CePO4@Cs prepared in Comparative Example 2;

[0033] Fig.10 a is Mn prepared in Comparative Example 1 5.64 TEM image of P3@Cs, b is Mn 5.64 EDS diagram of P3@Cs, c is Mn 5.64 HAADF-STEM image and corresponding element mapping of P3@Cs;

[0034] Fig.11 a is a TEM image of CePO4@Cs prepared in Comparative Example 2, b~c are high-resolution TEM images of CePO4@Cs, and d is a HAADF-STEM image of CePO4@Cs and a corresponding element mapping image;

[0035] Fig.12 Mn prepared in Example 1 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 Raman spectra of P3@Cs and CePO4@Cs prepared in Comparative Example 2;

[0036] Fig.13 The electrocatalyst Mn prepared in Examples 1 to 4 5.64 Raman spectrum of P3 / CePO4@Cs;

[0037] Fig.14 a is the CV curve of the products prepared in Example 1 and Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with N2 and O2, b is the LSV polarization curve of the products prepared in Example 1 and Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with O2, and c is the Tafel slope diagram of the products prepared in Example 1 and Examples 3 to 4;

[0038] Fig.15 In the figure, a is the CV curve of the products prepared in Example 1 and Comparative Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with N2 and O2, and b is the LSV polarization curve of the products prepared in Example 1 and Comparative Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with O2. DETAILED DESCRIPTION

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0040] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0044] The raw materials required for the embodiments of the present invention are all purchased from the market.

[0045] The room temperature / normal temperature in the present invention refers to 25±2°C.

[0046] Example 1 An oxygen reduction electrocatalyst Mn for zinc-air batteries 5.64 Preparation method of P3 / CePO4@Cs:

[0047] (1) Preparation of carbon sphere precursor: 25 μL of 1 mol / L potassium hydroxide solution was added to 40 mL of 0.5 mol / L glucose solution and stirred vigorously until a colorless and transparent solution was obtained. Then, the obtained solution was transferred to a stainless steel autoclave and subjected to hydrothermal reaction at 180°C for 6 h. The dark brown product was collected by centrifugation, washed with deionized water and ethanol for 3 times respectively, and finally dried at 60°C overnight to obtain a carbon sphere precursor;

[0048] (2) Preparation of Mn-Ce@Cs precursor: 100 mg of carbon sphere precursor, 6 mmol of Ce(NO3)2·6H2O and 6 mmol of MnCl2·4H2O were dispersed in a mixed solvent of 20 mL of ethanol and 40 mL of deionized water, stirred at room temperature for 8 h to form a uniform brown solution, and then centrifuged and dried to obtain a powder of Mn-Ce@Cs precursor.

[0049] (3) Oxygen reduction electrocatalyst Mn 5.64 Preparation of P3 / CePO4@Cs: 50 mg of Mn-Ce@Cs precursor was mixed with 100 mg of red phosphorus and ground. The obtained powder was placed at the bottom of a quartz tube and heated to 1000 °C at a heating rate of 5 °C / min under a nitrogen atmosphere. The mixture was kept warm for 2 h and then naturally cooled to room temperature before being taken out to obtain the oxygen reduction electrocatalyst Mn 5.64 P3 / CePO4@Cs(Ce1Mn1-P@Cs).

[0050] Example 2

[0051] The same as Example 1, except that in step (3), the temperature is increased to 800° C. at a heating rate of 5° C. / min under a nitrogen atmosphere and kept at this temperature for 2 h.

[0052] Example 3

[0053] The same as Example 1, except that in step (3), the temperature is increased to 900° C. at a heating rate of 5° C. / min under a nitrogen atmosphere and kept at this temperature for 2 h.

[0054] Example 4

[0055] The same as Example 1, except that in step (3), the temperature is increased to 1100° C. at a heating rate of 5° C. / min under a nitrogen atmosphere and kept at this temperature for 2 h.

[0056] Comparative Example 1 Electrocatalyst Mn 5.64 Preparation method of P3@Cs

[0057] (1) Preparation of carbon sphere precursor: same as in Example 1;

[0058] (2) Preparation of Mn@Cs: 100 mg of carbon sphere precursor and 12 mmol of MnCl2·4H2O were dispersed in a mixed solvent of 20 mL of ethanol and 40 mL of deionized water, stirred at room temperature for 8 h to form a uniform brown solution, which was then centrifuged and dried to obtain Mn@Cs powder.

[0059] (3) Mn 5.64 Preparation of P3@Cs: 50 mg of Mn@Cs precursor was mixed with 100 mg of red phosphorus and ground. The obtained powder was placed at the bottom of a quartz tube and heated to 1000 °C at a heating rate of 5 °C / min under a nitrogen atmosphere. The mixture was kept at this temperature for 2 h and then naturally cooled to room temperature before being taken out to obtain Mn@Cs. 5.64 P3@Cs.

[0060] Comparative Example 2 Preparation method of electrocatalyst CePO4@Cs

[0061] (1) Preparation of carbon sphere precursor: same as Example 1.

[0062] (2) Preparation of Ce@Cs: 100 mg of carbon sphere precursor and 12 mmol of Ce(NO3)2·6H2O were dispersed in 20 mL of ethanol and 40 mL of deionized water, stirred at room temperature for 8 h to form a uniform brown solution, which was then centrifuged and dried to obtain Ce@Cs powder;

[0063] (3) Preparation of CePO4@Cs: 50 mg of Ce@Cs precursor was mixed with 100 mg of red phosphorus and ground. The resulting powder was placed at the bottom of a quartz tube and heated to 1000°C at a heating rate of 5°C / min under a nitrogen atmosphere. The mixture was kept at this temperature for 2 h and then naturally cooled to room temperature before being taken out to obtain CePO4@Cs.

[0064] Comparative Example 3 Preparation method of electrocatalyst Ce1Mn3-P@Cs

[0065] The same as Example 1, except that the cerium salt and manganese salt added in step (2) are 3 mmol Ce(NO3)2·6H2O and 9 mmol MnCl2·4H2O, respectively.

[0066] Comparative Example 4 Preparation Method of Electrocatalyst Ce3Mn1-P@Cs

[0067] The same as Example 1, except that the cerium salt and manganese salt added in step (2) are 9 mmol Ce(NO3)2·6H2O and 3 mmol MnCl2·4H2O, respectively.

[0068] Effect Example 1

[0069] Figure 1 a is the preparation of oxygen reduction electrocatalyst Mn in Example 1 5.64Basic flow chart of P3 / CePO4@Cs, b is the electrocatalyst Mn prepared in Example 1 5.64 The XRD diagram of P3 / CePO4@Cs, c is the EPR spectrum of the electrocatalysts prepared in Example 1 and Comparative Examples 1-2, d is the N2 adsorption-desorption isotherm and pore size distribution diagram of the electrocatalyst prepared in Example 1, and e is the Mn prepared in Example 1. 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 Comparison of contact angles of P3@Cs and CePO4@Cs prepared in comparative example 2.

[0070] from Figure 1 In a, we can see that the electrocatalyst Mn 5.64 The preparation method of P3 / CePO4@Cs is simple and the material is novel; Figure 1 In b, it can be seen that the electrocatalyst Mn prepared in Example 1 5.64 The constituent phase of P3 / CePO4@Cs is Mn 5.64 P3 and CePO4; from Figure 1 In c, it can be seen that the Mn prepared in Example 1 5.64 There are phosphorus (P) vacancies in P3 / CePO4. The formation of P vacancies can promote electron delocalization, enhance carrier mobility, accelerate charge transfer, strengthen oxygen adsorption, and regulate the adsorption energy of intermediates, thereby improving the ORR electrocatalytic performance. Figure 1 In d, it can be seen that the electrocatalyst Mn prepared in Example 1 5.64 P3 / CePO4@Cs has a high specific surface area, which can effectively promote the interaction between electrolyte and active sites, accelerate the ion transport in the ORR process, and thus improve the catalytic yield. Figure 1 As can be seen in e, the electrocatalyst Mn prepared in Example 1 5.64 The solution contact angle of P3 / CePO4@Cs is better than that of Mn prepared in Example 1. 5.64 The P3@Cs and CePO4@Cs prepared in comparative example 2 are smaller, indicating that the product prepared in example 1 has better wettability, which is beneficial to the penetration of electrolyte and the transfer of ions, thereby significantly improving the electrochemical ORR efficiency at the interface.

[0071] Effect Example 2

[0072] The SEM image of the carbon sphere precursor prepared in Example 1 of the present invention is shown in Figure 2 ;from Figure 2 It can be seen that the carbon sphere precursor prepared using glucose in Example 1 presents a spherical structure with a smooth surface.

[0073] Figure 3 a is Mn 5.64 SEM image of P3 / CePO4@Cs, b is Mn5.64 TEM images of P3 / CePO4@Cs, c~e are Mn 5.64 High-resolution TEM image of P3 / CePO4@Cs, f is Mn 5.64 HAADF-STEM image of P3 / CePO4@Cs and corresponding element mapping.

[0074] from Figure 3 It can be seen from a that the Mn obtained after high temperature calcination 5.64 P3 / CePO4@Cs still maintains the structure of carbon spheres. Figure 3 b further shows the Mn prepared in Example 1 5.64 The morphology of P3 / CePO4@Cs and Figure 3 The c in the figure indicates Mn 5.64 The interface between P3 and CePO4. Figure 3 As can be seen in d and e, it is further confirmed that the Mn prepared in Example 1 5.64 There are phosphorus vacancies on the surface of P3 / CePO4@Cs. The (110) surface of CePO4 and Mn 5.64 The (210) plane of P3 has obvious lattice fringes, and the interplanar spacings are 0.354nm and 0.199nm respectively. Figure 3 As can be seen in middle f, C, O, P, Ce and Mn are evenly distributed in the nanospheres.

[0075] Example 1: Mn 5.64 The EDS spectrum of P3 / CePO4@Cs is shown in Figure 4 , Figure 4 The existence of C, O, P, Ce and Mn elements was further confirmed.

[0076] Effect Example 3

[0077] Mn prepared in Example 1 of the present invention 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 The XPS graphs of P3@Cs and CePO4@Cs prepared in Comparative Example 2 are shown in Figure 5 .

[0078] Figure 5In which a is the UPS diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, b is the band structure diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, c is the XPS diagram of the product prepared in Example 1 in the C1s region, d is the XPS diagram of the products prepared in Example 1 and Comparative Example 2 in the Ce 3d region, e is the XPS diagram of the products prepared in Example 1 and Comparative Example 1 in the Mn 2p region, f is the XPS diagram of the products prepared in Example 1 and Comparative Examples 1 to 2 in the P 2p region, and g is the XPS diagram of the products prepared in Example 1 and Comparative Example 2 in the O1s region.

[0079] Ultraviolet photoelectron spectroscopy (UPS) was used to deeply analyze the electronic properties of the synthesized samples to study their enhanced intrinsic activity. Figure 5 As shown in a, Mn 5.64 P3 / CePO4@Cs、Mn 5.64 The work functions (ΔΦ) of P3@Cs and CePO4@Cs are 4.41, 4.54, and 4.30 eV, respectively. 5.64 The valence band maximum (E v ) are 2.60 and 3.43 eV respectively ( Figure 5 b), and Mn 5.64 The band gap of P3 / CePO4@Cs is moderate, 3.19 eV. d ) theory, the d-band center is close to the Fermi level (E f ) will lead to an increase in the number of empty antibonding states and an increase in the adsorption force of the reaction intermediates. 5.64 P3 / CePO4@Cs is beneficial in providing optimized active sites for the adsorption and desorption of oxygen-containing intermediates. Figure 5 c shows that Mn prepared in Example 1 5.64 The C1s spectrum of P3 / CePO4@Cs shows four peaks, namely C=C (284.0 eV), CC (284.5 eV), CO (286.4 eV) and C=O (289.8 eV). In the Ce 3d XPS spectrum, μ and v represent Ce 3d 5 / 2 and Ce 3d 3 / 2 The spin-orbit coupling of Mn 5.64 The μ2 / μ3 peaks of Ce3d in P3 / CePO4@Cs shifted positively by 0.45 eV and 0.56 eV, respectively. Figure 3 d). Figure 5 Mn 5.64 The Mn 2p peak of P3 / CePO4@Cs is relatively 5.64P3@Cs exhibits a negative shift (about 0.28 eV), indicating that CePO4 modulation enhances the electron density of Mn at the interface. 5.64 P3, consistent with the UPS results. Figure 5 The XPS spectrum of P 2p in f shows two main peaks with binding energies of 129.5 and 130.5 eV, corresponding to P 2p 3 / 2 and P 2p 1 / 2 In addition, the P 2p peak exhibits a peak at 132.6 eV, indicating the formation of P-O bonds due to surface oxidation. Figure 5 In g, the high-resolution O1s spectrum shows three different types of oxygen: metallic oxygen (529.7 eV), OC=O (531.4 eV) and surface adsorbed oxygen (533.1 eV).

[0080] Effect Example 4

[0081] Determination of Mn prepared in Example 1 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 The electrochemical performance of P3@Cs, CePO4@Cs prepared in Comparative Example 2, and commercial Pt / C (purchased from AlfaAesar) are shown in Figure 6 .

[0082] The electrochemical performance test method is as follows:

[0083] The measurement was performed using a CHI 760E electrochemical workstation. The workstation used a three-electrode system, in which a graphite rod electrode was used as an auxiliary electrode and an Ag / AgCl electrode (saturated potassium chloride) was used as a reference electrode. The electrocatalysts used were Mn prepared in Example 1. 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 P3@Cs, CePO4@Cs prepared in Comparative Example 2, and commercial Pt / C: 2 mg of the electrocatalyst was mixed with 200 μL of isopropanol, 100 μL of deionized water, and 5 μL of Nafion, and ultrasonicated for 1 h to form a homogeneous electrocatalyst ink. 20 μL of the electrocatalyst ink was dropped onto a rotating disk electrode and allowed to dry naturally to obtain a catalyst electrode. Solution saturation: Before the test, the electrolyte was continuously bubbled for 30 min, and N2 or O2 gas was used to continuously saturate the solution with N2 or O2. During the test, gas bubbling continued to keep the solution saturated with N2 or O2. Reference electrode calibration: All potentials were measured with respect to RHE. RHE calibration was performed in a 0.1 mol / L high-purity potassium hydroxide solution that was saturated with hydrogen.

[0084] (1) Cyclic voltammetry (CV) measurements were first performed in a 0.1 mol / L potassium hydroxide solution saturated with N2 or O2, with a potential range of -0.9 to 0.2 V and a scan rate of 30 mV compared to the reference electrode.

[0085] (2) Linear sweep voltammetry (LSV) curves: The LSV curves of different catalysts in 0.1 mol / L potassium hydroxide electrolyte at a rotation speed of 1600 rpm were obtained. In addition, the Mn prepared in Example 1 was also obtained. 5.64 LSV curves of P3 / CePO4@Cs catalyst at different rotation speeds (400-1600rpm).

[0086] (3) Tafel slope: calculated by the Tafel equation. The Tafel equation quantitatively describes the relationship between the electrochemical reaction rate and the potential:

[0087] Where η is the electrode overpotential, b is the Tafel slope, j is the current density, and j0 is the exchange current density.

[0088] (4) Methanol tolerance test: The methanol tolerance test was conducted at a rotation speed of 1600 rpm using 0.1 mol / L potassium hydroxide saturated with oxygen.

[0089] (5) RRDE test: The H2O2 yield (%) and the number of electron transfers (n) in ORR were measured by RRDE at 1600 rpm, and the formula is:

[0090] Among them, i D is the disk current, i R is the platinum ring current, and N is the collection efficiency of the platinum ring (N=0.37).

[0091] Figure 6 In the figure, a is the CV curve of the products prepared in Example 1 and Comparative Examples 1 to 2 in a 0.1 mol / L KOH solution saturated with N2 and O2, b is the LSV polarization curve of the products prepared in Example 1, Comparative Examples 1 to 2 and commercial Pt / C in a 0.1 mol / L KOH solution saturated with O2, c is the Tafel diagram of the products prepared in Example 1 and Comparative Examples 1 to 2, and d is the half-wave potential (E) of the products prepared in Example 1 and Comparative Examples 1 to 2 at 0.8 V. 1 / 2 ) and kinetic current density (J k ), e is the double layer capacitance (C dl ) value, f is the oxygen reduction onset potential and half-wave potential (E 1 / 2), g is the H2O2 yield (%) and the number of electron transfers (n) of the products prepared in Example 1 and Comparative Examples 1 to 2, h is the methanol tolerance test result of the product prepared in Example 1 and commercial Pt / C, i is the stability test result of the products prepared in Example 1 and Comparative Examples 1 to 2 in an O2-saturated 0.1 mol / L KOH solution (at 1600 rpm).

[0092] Table 1

[0093]

[0094] from Figure 6 In a, we can see that Mn 5.64 Compared with Mn 5.64 The cathode peak of P3 / CePO4@Cs is more positive, indicating that it has better ORR activity.

[0095] from Figure 6 As can be seen in b, Mn 5.64 P3 / CePO4@Cs has excellent ORR activity, and its onset potential (E onset ) and limiting current density (j L ) exceeds the catalysts prepared in Comparative Examples 1-2 and is closely related to commercial Pt / C.

[0096] from Figure 6 In c, we can see that Mn 5.64 The Tafel slope of P3 / CePO4@Cs is 143 mV·dec -1 , lower than CePO4@Cs(161mV·dec -1 ), indicating that the Mn prepared by combining with Mn element 5.64 P3 / CePO4@Cs can reduce the Tafel slope of CePO4@Cs and improve the activity of ORR reaction.

[0097] from Figure 6 It can be seen from the figure that Mn 5.64 The half-wave potential value of P3 / CePO4@Cs is the highest, reaching 0.8V, exceeding that of Mn 5.64 P3@Cs (0.74 V) and CePO4@Cs (0.76 V), highlighting their excellent ORR performance.

[0098] from Figure 6 It can be seen from e that Mn 5.64 P3 / CePO4@Cs and CePO4@Cs (2.3mF·cm -2 ), Mn 5.64 P3@Cs(1.4mF·cm -2) has the highest C dl Value 4.2mF·cm -2 Mn 5.64 P3 / CePO4@Cs has more ORR reaction active sites.

[0099] from Figure 6 It can be seen from f that Mn 5.64 P3 / CePO4@Cs has a high oxygen reduction onset potential (E onset ) and half-wave potential (E 1 / 2 ) has a higher oxygen reduction onset potential and half-wave potential.

[0100] from Figure 6 It can be seen from g that Mn 5.64 P3 / CePO4@Cs has a low H2O2 yield (<25%) and a high electron transfer number (3.95) in the potential range of 0.2-0.8 V, indicating that the Mn prepared in Example 1 5.64 The oxygen reduction reaction of P3 / CePO4@Cs tends to be a four-electron reduction pathway.

[0101] The stability and methanol resistance were evaluated in an O2-saturated 0.1 mol / L KOH electrolyte at 1600 rpm. When methanol (the concentration of methanol in KOH is 3 mol / L) was rapidly injected into the electrolyte, the current density of commercial Pt / C decreased significantly, while that of Mn 5.64 P3 / CePO4@Cs can maintain a constant current density, indicating that Mn 5.64 P3 / CePO4@Cs has excellent methanol resistance ( Figure 6 h); from Figure 6 It can be seen from i that Mn 5.64 The current density of P3 / CePO4@Cs can still maintain 97% of its initial value after about 18 h, while CePO4@Cs can only maintain 90% after about 9 h. 5.64 P3@Cs can only maintain 73% after about 9 hours, indicating that Mn 5.64 P3 / CePO4@Cs has good stability.

[0102] Effect Example 5

[0103] Assembly and testing of zinc-air batteries (aqueous ZAB):

[0104] 2 mg Mn 5.64The catalyst P3 / CePO4@Cs+2mg RuO2 (mass ratio of 1:1) was dispersed in a mixed solution of 200μL ethanol, 200μL deionized water and 10μL 5% Nafion. After ultrasonication for 30min, the catalyst ink was obtained. The catalyst ink was dropped on a 1cm×1cm carbon cloth and dried at room temperature as an air cathode. The zinc foil was used as the anode. 6.0mol / L KOH and 0.2mol / L Zn(A) were used as the cathode. C )2 mixed solution was used as the electrolyte of ZAB, and commercial Pt / C+RuO2 was prepared as a control. Mn was measured using a CHI 760E electrochemical workstation 5.64 Polarization curves and open circuit voltage (OCV) of ZAB of P3 / CePO4@Cs were obtained. The stability of ZAB was tested using the RAND battery test system. The current density of each charge-discharge cycle was 5 mA cm -2 , lasting 20 minutes.

[0105] The performance of the zinc-air battery prepared in this example was measured and the results are shown in Figure 7 .

[0106] Figure 7 In the figure, a is a schematic diagram of the configuration of the zinc-air battery, b is an open circuit voltage (OCV) diagram of the zinc-air battery, c is a discharge polarization curve and corresponding power density of the zinc-air battery, d is a specific capacity diagram of the zinc-air battery, e is a discharge curve of the zinc-air battery at different current densities, and f is a graph of the Mn in Example 1. 5.64 The LED panel image lit by the ZAB assembled with P3 / CePO4@Cs; g is the comparison of the power density and specific capacity of the zinc-air battery prepared in this example with other recently reported ORR catalysts (see Table 2); h is the power density and specific capacity of the zinc-air battery at 5 mA cm -2 Electrostatic cycles under (20min each cycle).

[0107] Table 2

[0108] Catalysts Specific capacity Power density DOI <![CDATA[Mn 5.64 P3 / CePO4@Cs]]> 708 168 This work <![CDATA[Cu3P / MoP@C]]> 704 156 10.1016 / j.apcatb.2021.120415 CoP / HNBs@NCL-2 728.8 139.8 10.1016 / j.cej.2023.146154 <![CDATA[CoCe-600N2]]> 634 116.8 10.1039 / C9TA00302A <![CDATA[Fe2P / NPCs]]> 691.0 128.38 10.1016 / j.jpowsour.2021.230006 <![CDATA[CeO2@NC-900]]> 585.1 118.2 10.1016 / j.jcis.2020.06.040 Co / MnO@N,S-CNT / NFs 726.6 120.7 10.1016 / j.apcatb.2021.120281 FeNSPC1000 702 91 10.1016 / j.est.2023.107950

[0109] from Figure 7 From a to b, we can see that the use of Mn 5.64 The aqueous ZAB constructed with P3 / CePO4@Cs exhibits an open circuit voltage exceeding the OCV of commercial Pt / C. 5.64 The aqueous ZAB constructed with P3 / CePO4@Cs is able to power the “GXNU” LED screen (f).

[0110] from Figure 7 It can be seen from c that Mn 5.64 The peak power density of P3 / CePO4@Cs is 168 mW cm -2, which is better than commercial Pt / C (129mW·cm -2 ).

[0111] from Figure 7 It can be seen from the figure that Mn 5.64 Specific capacity of P3 / CePO4@Cs Higher than commercial Pt / C-based water-based This further confirmed its excellent discharge performance.

[0112] from Figure 7 It can be seen from e that Mn 5.64 P3 / CePO4@Cs has excellent rate performance, even at 50 mA cm -2 At high current density, the discharge voltage can also be maintained above 0.8V. When the current density is restored to 2mA·cm -2 When the current density is 0.50V, there is only a small voltage loss (0.04V) compared with the initial current density.

[0113] from Figure 7 It can be seen from g that Mn 5.64 P3 / CePO4@Cs as air cathode has better power density and specific capacity compared with other recently reported ORR catalysts.

[0114] from Figure 7 It can be seen from h that Mn 5.64 After 400 h of continuous operation, the voltage retention rate of P3 / CePO4@Cs is as high as 90%, while the voltage retention rate of commercial Pt / C begins to decay rapidly. After 120 h of operation, the voltage retention rate is only 82%, indicating that Mn 5.64 P3 / CePO4@Cs has good stability.

[0115] Effect Example 6

[0116] Figure 8 In the figure, a is the XRD graph of Mn5.64P3@Cs prepared in comparative example 1, and b is the XRD graph of CePO4@Cs prepared in comparative example 2.

[0117] from Figure 8 It can be seen that Mn 5.64 The XRD patterns of P3@Cs and CePO4@Cs are respectively 5.64 The spectra of P3 (JCPDS: 30-0823) and CePO4 (JCPDS: 04-0632) are consistent, indicating that Mn 5.64 Successful synthesis of P3 and CePO4.

[0118] Fig. 9 a is Mn prepared in Comparative Example 1 5.64a is the N2 adsorption-desorption isotherm and pore size distribution diagram of P3@Cs, b is the N2 adsorption-desorption isotherm and pore size distribution diagram of CePO4@Cs prepared in comparative example 2.

[0119] from Figure 1 d and Fig. 9 It can be seen that the Mn prepared in Example 1 of the present invention 5.64 P3 / CePO4@Cs has a larger specific surface area than the products prepared in Comparative Examples 1 to 2, and can expose more active sites, thereby improving the catalytic activity.

[0120] Fig.10 In the figure, a is Mn prepared in Comparative Example 1. 5.64 TEM image of P3@Cs, b is Mn 5.64 EDS diagram of P3@Cs, c is Mn 5.64 HAADF-STEM image of P3@Cs and corresponding element mapping.

[0121] from Fig.10 As can be seen in a, Mn and P are successfully loaded on the surface of carbon spheres. Fig.10 b to c further confirm that the Mn prepared in Comparative Example 1 5.64 P3@Cs contains C, P, and Mn elements.

[0122] Fig.11 In the figure, a is the TEM image of CePO4@Cs prepared in Comparative Example 2, b~c are high-resolution TEM images of CePO4@Cs, and d is the HAADF-STEM image of CePO4@Cs and the corresponding element mapping image.

[0123] from Fig.11 As can be seen in a, Ce and P are successfully loaded on the surface of carbon spheres. Fig.11 It can be seen from b to c that the (110) of CePO4 prepared in Comparative Example 2 has obvious lattice fringes, and its interplanar spacing is 0.354nm, which is consistent with the results measured for the product prepared in Example 1, indicating that CePO4 exists in both Example 1 and Comparative Example 2. Fig.11 Figure d further confirms the presence of Ce, P, C, and O elements in CePO4@Cs prepared in Comparative Example 2.

[0124] Example 1: Mn 5.64 P3 / CePO4@Cs, Mn prepared in Comparative Example 1 5.64 The Raman spectra of P3@Cs and CePO4@Cs prepared in Comparative Example 2 are shown in Fig.12 .

[0125] from Fig.12 It can be seen that the catalysts prepared in Example 1 and Comparative Examples 1 to 2 have a-1 and 1589cm -1 There are two different peaks at the center, namely D band (defect) and G band (graphitization). The peak intensity ratio of the DG band of the products prepared in Example 1 and Comparative Examples 1 to 2 is (I D / I G ) are 1.18, 0.98, and 1.24, respectively, indicating that the Mn prepared in Example 1 5.64 P3 / CePO4@Cs achieves a proper balance between defect formation and graphitization, which is beneficial to enhance the ORR activity of the electrocatalyst.

[0126] Electrocatalyst Mn prepared in Examples 1 to 4 5.64 Raman spectrum of P3 / CePO4@Cs is shown in Fig.13 .

[0127] from Fig.13 It can be seen that in Example 1, Mn was prepared at 1000°C. 5.64 P3 / CePO4@Cs and Mn prepared at 800℃, 900℃ and 1100℃ respectively in Examples 2 to 4 5.64 The DG band peak intensity ratio of P3 / CePO4@Cs (I D / I G ) are 0.96, 1.28, 1.19, and 0.80, respectively, which also shows that the Mn prepared in Example 1 at 1000°C 5.64 P3 / CePO4@Cs achieves a proper balance between defect formation and graphitization, which is beneficial to enhance the ORR activity of the catalyst.

[0128] The electrochemical properties of the product prepared in Example 3 at 900°C, the product prepared in Example 1 at 1000°C, and the product prepared in Example 4 at 1100°C are shown in FIG. Fig.14 .

[0129] Fig.14 In the figure, a is the CV curve of the products prepared in Example 1 and Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with N2 and O2, b is the LSV polarization curve of the products prepared in Example 1 and Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with O2, and c is the Tafel slope diagram of the products prepared in Example 1 and Examples 3 to 4.

[0130] from Fig.14 It can be seen that the sample obtained when the calcination temperature is 1000℃ has the best ORR performance, including the most positive reduction potential ( Fig.14 a), the maximum limiting current density and the maximum half-wave potential ( Fig.14 b), the smaller Tafel slope ( Fig.14(c) It is confirmed that the catalyst has the best ORR performance at 1000 °C.

[0131] The electrochemical properties of Ce1Mn1-P@Cs prepared in Example 1, Ce1Mn3-P@Cs prepared in Comparative Example 3, and Ce3Mn1-P@Cs prepared in Comparative Example 4 are shown in Fig.15 .

[0132] Fig.15 In the figure, a is the CV curve of the products prepared in Example 1 and Comparative Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with N2 and O2, and b is the LSV polarization curve of the products prepared in Example 1 and Comparative Examples 3 to 4 in a 0.1 mol / L KOH solution saturated with O2.

[0133] from Fig.15 It can be seen that when the dosage ratio of Ce(NO3)2·6H2O and MnCl2·4H2O is 1:1, the sample obtained has the best ORR performance, including the most positive reduction potential ( Fig.15 a), the maximum limiting current density and the maximum half-wave potential ( Fig.15 (b)

[0134] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. An oxygen reduction electrocatalyst Mn for zinc-air batteries 5.64 The preparation method of P3 / CePO4@Cs is characterized in that: The following steps are involved: The carbon sphere precursor, cerium salt and manganese salt are mixed in a solvent and stirred at room temperature to obtain a Mn-Ce@Cs precursor; the Mn-Ce@Cs precursor is phosphated under an inert gas atmosphere to obtain the oxygen reduction electrocatalyst Mn 5.64 P3 / CePO4@Cs.

2. The preparation method according to claim 1, characterized in that: The usage ratio of the carbon sphere precursor, cerium salt and manganese salt is 100 mg: 6 mmol: 6 mmol.

3. The preparation method according to claim 2, characterized in that: The cerium salt is Ce(NO3)2·6H2O, and the manganese salt is MnCl2·4H2O.

4. The preparation method according to claim 1, characterized in that: The solvent is a mixed solvent of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1:

2.

5. The preparation method according to claim 1, characterized in that: The stirring time is 8h.

6. The preparation method according to claim 1, characterized in that: The phosphating treatment is to mix and grind the Mn-Ce@Cs precursor and red phosphorus, and then keep the mixture at 800-1100° C. for 2 hours.

7. The preparation method according to claim 6, characterized in that: The mass ratio of the Mn-Ce@Cs precursor to red phosphorus is 1:

2.

8. An oxygen reduction electrocatalyst Mn for zinc-air batteries 5.64 P3 / CePO4@Cs, characterized in that It is prepared by the preparation method according to any one of claims 1 to 7.

9. An oxygen reduction electrocatalyst Mn for a zinc-air battery as claimed in claim 8 5.64 Application of P3 / CePO4@Cs in catalytic oxygen reduction of zinc-air batteries.