Photo-thermal electrolyte, application and preparation method thereof, and photo-thermal all-solid-state lithium metal battery
By combining polyethylene oxide with lithiated poly(3,4-hydroxythiophene) to form a photothermolyte, the problem of difficulty in operating in a low-temperature environment is solved, and high temperature in a low-temperature environment is achieved The magnification cycle and electrochemical performance improve, avoiding additional power loss.
Patent Information
- Application Number
- CN202411040990.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
AI Technical Summary
Existing PEO-based polymer solid-state batteries are difficult to operate properly in low temperature environments, and existing solutions require additional electric heating devices for electrically assisted heating, resulting in electrical energy loss.
Using photothermal electrolyte, polyethylene oxide (PEO), lithium salt and lithiated poly(3,4-hydroxythiophene) composite materials can increase the operating temperature of the battery through photothermal conversion, achieving improved electrochemical performance and enhanced cycle stability .
High-speed cycles can be achieved without additional power loss in sub-zero low temperature environments, which improves the electrochemical performance and cycle stability of the battery and is suitable for low-temperature environments.
Smart Images

Figure CN119050462A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of battery technology, and specifically relates to a photothermal electrolyte and its application and preparation method, and also relates to a photothermal all-solid-state lithium metal battery including the photothermal electrolyte. Background Art
[0002] More than two-thirds of my country's area has an average winter temperature below 0°C, and related applications in the fields of aerospace and military equipment will face more extreme temperature environments. Therefore, as the application scope of electronic equipment continues to expand, the market will not only require solid-state batteries to have excellent electrochemical properties, but will also place higher demands on the environmental adaptability of solid-state batteries. In other words, the polymer-based solid electrolytes in solid-state batteries must meet the requirements of high reliability service under low temperature conditions to achieve commercial applications.
[0003] Among the common polymer-based solid electrolytes, PEO polymer electrolyte has a higher electrical conductivity, and the research and development and improvement of its electrolyte system has good application prospects.
[0004] In the art, there is a technical solution for effectively improving the electrochemical performance of polyoxyethylene (PEO) polymer electrolyte by compounding PEO with fillers, which enables the operation of PEO-based solid-state batteries at high temperatures or room temperatures, as follows:
[0005] Patent document with publication number CN 117976959A discloses a composite solid electrolyte and its preparation method and application. The composite solid electrolyte includes: a composite electrolyte and fluorinated boron nitride nanosheets; the fluorinated boron nitride nanosheets are coated on the surface of the composite electrolyte; the composite electrolyte includes a polymer electrolyte and a lithium salt.
[0006] Patent document with publication number CN 117254095A discloses an organic-inorganic composite solid electrolyte material and an organic-inorganic solid electrolyte composite membrane and a coated composite membrane using the same, wherein the organic-inorganic composite solid electrolyte material comprises the following components: inorganic ion conductive nanoparticles coated with polydopamine and a polymer electrolyte matrix; the weight ratio of the dopamine-coated inorganic ion conductive nanoparticles and the polymer electrolyte matrix is 7.5-8.5:1.5-2.5.
[0007] However, the PEO-based polymer solid-state battery produced by the above-mentioned prior art is still difficult to operate normally in a lower temperature environment. In order to realize the use of PEO-based polymers in sub-zero low temperature environments, the most direct and effective means is to increase the working temperature of the PEO-based solid-state battery through electric auxiliary heating, but this method requires the installation of an additional electric heating device.
[0008] In summary, the present invention aims to develop a PEO polymer electrolyte that does not require additional power consumption and can be heated quickly. Summary of the invention
[0009] In response to the problems in the related technology, the present invention proposes a photothermal electrolyte and its application, preparation method, and photothermal all-solid-state lithium metal battery to overcome the above-mentioned technical problems existing in the existing related technology.
[0010] The technical solution of the present invention is achieved in this way:
[0011] A photothermal electrolyte, wherein the raw materials for preparing the electrolyte include polyethylene oxide (PEO), lithium salt and filler;
[0012] The filler is lithiated poly(3,4-hydroxythiophene).
[0013] Among the many methods of obtaining thermal energy, photothermal conversion has significant advantages such as high efficiency and strong economy. Therefore, the present invention composites the polymer PEO with a photothermal material, namely, lithiated poly(3,4-hydroxythiophene). On the one hand, the photothermal material can play the role of a filler to improve the electrochemical performance, thereby effectively improving the electrochemical performance and cycle stability of the PEO polymer electrolyte. On the other hand, the composite polymer solid electrolyte can realize photothermal conversion characteristics, and the battery operating temperature can be increased through photothermal conversion, thereby further improving the battery performance. That is, the present invention realizes the dual functionality of electrochemical performance improvement and photothermal conversion by composite the polymer electrolyte PEO with a photothermal filler, thereby solving the problem that the PEO-based polymer electrolyte is not suitable for application in low-temperature environments.
[0014] The photothermal electrolyte prepared by the present invention has a photothermal conversion effect under the action of light, and the light source of the light can be sunlight, xenon lamp, laser, etc.
[0015] Preferably, the mass ratio of the polyethylene oxide, the lithium salt and the lithiated poly(3,4-hydroxythiophene) is 100:60:2.5-10.
[0016] Specifically, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0017] The present invention also discloses a method for preparing the above-mentioned photothermal electrolyte, comprising the following steps:
[0018] 1) In an inert gas atmosphere, polyethylene oxide, lithium salt and lithiated poly(3,4-hydroxythiophene) are placed in an organic solvent and mixed uniformly;
[0019] 2) The solution prepared in step 1) is spread out and then dried to form a film, thereby obtaining a film-like photothermal electrolyte.
[0020] Preferably, in step 1), the inert gas is argon, and the organic solvent is anhydrous acetonitrile.
[0021] Preferably, the drying operation in step 2) is specifically as follows: firstly naturally drying to form a film, and then placing in a vacuum environment at 55-65° C. to continue drying until the residual organic solvent is removed.
[0022] The present invention also discloses the application of the above-mentioned photothermal electrolyte in solid-state batteries. High energy density lithium metal solid-state batteries are strong competitors for the next generation of energy storage systems. Therefore, the present invention focuses on the application of the above-mentioned photothermal electrolyte in lithium metal solid-state batteries. It should be noted that the photothermal electrolyte prepared by the present invention can also be used in the field of photothermal conversion products.
[0023] A photothermal all-solid-state lithium metal battery comprises the above-mentioned photothermal electrolyte.
[0024] Preferably, the photothermal all-solid-state lithium metal battery is stacked with a lithium metal negative electrode sheet, the photothermal electrolyte, a positive electrode sheet and the photothermal electrolyte in sequence from bottom to top.
[0025] Specifically, the thickness of the photothermal electrolyte is 90-100 μm.
[0026] The photothermal all-solid-state lithium metal battery prepared by the present invention not only has excellent electrochemical properties, but can also operate in a sub-zero low temperature environment or a high temperature environment.
[0027] The present invention also discloses a method for preparing the positive electrode sheet, comprising the following steps:
[0028] S1. Weigh the positive electrode material, polyvinylidene fluoride and carbon black conductor in a mass ratio of 7.5-8.5:0.5-1.5:0.5-1.5, grind and mix;
[0029] S2, adding an appropriate amount of solvent to the mixture ground in S1, and continuing to grind until a uniform electrode slurry is formed;
[0030] S3, evenly coating the electrode slurry in S2 on the carbon-coated aluminum foil to form a uniform electrode coating, and performing vacuum drying at a temperature of 60 to 80° C. for 12 to 24 hours;
[0031] S4, punching the sheet material dried in S3 to make the positive electrode sheet.
[0032] Preferably, the positive electrode material is LiFePO4 or LiNi 0.5 Co 0.2 Mn 0.3 O2.
[0033] The present invention also discloses a solar thermal all-solid-state lithium metal battery capable of operating at sub-zero temperatures, comprising the above-mentioned solar thermal all-solid-state lithium metal battery;
[0034] The photothermal all-solid-state lithium metal battery adopts transparent packaging to achieve the goal of directly applying photothermal effect to the interior of the battery and increasing the operating temperature.
[0035] Specifically, the transparent package uses polyethylene terephthalate transparent film (PET transparent film) as the outer packaging of the photothermal all-solid-state lithium metal battery.
[0036] The operating temperature of the photothermal all-solid-state lithium metal battery produced by the present invention is increased without the need for additional power loss, and a high-rate cycle of the PEO-based solid-state battery in a sub-zero low-temperature environment is achieved, which has certain application value in the low-temperature application of polyethylene oxide-based solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram of the structure of the photothermal all-solid-state lithium metal battery of the present invention and its transparent packaging diagram;
[0038] Figure 2 This is a surface microscopic morphology of the photothermal electrolyte of the present invention;
[0039] Figure 3 This is a cross-sectional microscopic morphology diagram of the photothermal electrolyte of the present invention;
[0040] Figure 4 The room temperature lithium ion conductivity test graphs of Examples 1 to 4 and Comparative Example 1;
[0041] Figure 5 This is a linear sweep voltammetry curve obtained by testing Example 2;
[0042] Figure 6 This is a temperature rise curve diagram obtained from the light and heat performance test of Example 2 and Comparative Example 1;
[0043] Figure 7 This is a charge and discharge cycle performance diagram obtained from the cycle performance test of Example 2;
[0044] Figure 8 is the cycle performance diagram of Example 5;
[0045] Fig. 9 Graphs showing the cycle performance of Example 6 and Comparative Example 2;
[0046] Fig.10 This is a temperature rise curve diagram of Example 7 under xenon lamp irradiation;
[0047] Fig.11 This is the charge and discharge curve of Example 7 under xenon lamp irradiation. DETAILED DESCRIPTION
[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] In the following examples and comparative examples, the molecular weight of PEO is 600,000, and the purity of the used LiTFSI is greater than 99%.
[0050] Example 1
[0051] A photothermal electrolyte, the preparation method is as follows:
[0052] 1) In an argon glove box, polyethylene oxide (PEO), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithiated poly(3,4-hydroxythiophene) were dissolved in 20 ml of anhydrous acetonitrile at a mass ratio of 100:60:2.5 (i.e., 1000 mg:600 mg:25 mg) and stirred for 12 h until uniform;
[0053] 3) The solution obtained in step 2) is cast into a polytetrafluoroethylene mold and dried naturally to form a film, and then placed in a vacuum environment at 60° C. to dry for 12 hours to remove the residual organic solvent, thereby obtaining a film-like photothermal electrolyte.
[0054] Example 2
[0055] Compared with Example 1, the mass ratio of PEO, LiTFSI and lithiated poly(3,4-hydroxythiophene) in this example is 100:60:5; the other operations are the same.
[0056] Example 3
[0057] Compared with Example 1, the mass ratio of PEO, LiTFSI and lithiated poly(3,4-hydroxythiophene) in this example is 100:60:7.5; the rest of the operations are the same.
[0058] Example 4
[0059] Compared with Example 1, the mass ratio of PEO, LiTFSI and lithiated poly(3,4-hydroxythiophene) in this example is 100:60:10; the rest of the operations are the same.
[0060] Example 5
[0061] A photothermal all-solid-state lithium metal battery, the preparation method comprising the following steps:
[0062] A. Preparation of positive electrode sheet:
[0063] S1. Lithium iron phosphate (LiFePO4), polyvinylidene fluoride (PVDF) and carbon black conductive agent (Super P) were weighed in a mass ratio of 8:1:1, put into a mortar, and manually ground for 30 minutes.
[0064] S2. Add an appropriate amount of N-methylpyrrolidone (NMP) to the mixture ground in S1, and continue to grind manually for 30 minutes until a uniform electrode slurry is formed.
[0065] S3. The electrode slurry in S2 is evenly coated on the carbon-coated aluminum foil to form a uniform electrode coating, and then transferred to a vacuum drying oven for vacuum drying at 80° C. for 18 hours.
[0066] S4. Punch the electrode sheet dried in S3 to make a round sheet with a diameter of 12 mm, which is the LiFePO4 positive electrode sheet.
[0067] B. Assembly: Refer to Figure 1 , stacked from bottom to top in sequence are a lithium metal negative electrode sheet 3, the photothermal electrolyte membrane 1 prepared in Example 2, a LiFePO4 positive electrode sheet 2 and the photothermal electrolyte membrane 1 prepared in Example 2.
[0068] Example 6
[0069] A photothermal all-solid-state lithium metal battery. The difference between this embodiment and embodiment 5 is that LiFePO4 is replaced by LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523); the rest of the operations are the same as in Example 5.
[0070] Example 7
[0071] Reference Figure 1 , a solar thermal all-solid-state lithium metal battery that can operate at sub-zero temperatures, specifically, transparently encapsulating Example 5, and the outer packaging used for the transparent encapsulation is a PET transparent film 4.
[0072] Comparative Example 1
[0073] Compared with Example 2, this comparative example does not contain lithiated poly(3,4-hydroxythiophene); the remaining operations are the same to prepare an electrolyte membrane.
[0074] Comparative Example 2
[0075] Compared with Example 7, this comparative example adopts the electrolyte membrane prepared in Comparative Example 1; the remaining operations are the same to prepare a packaged battery.
[0076] Performance Testing
[0077] 1. Microscopic morphology observation
[0078] Since the microscopic morphologies of the photothermal electrolyte membranes prepared in Examples 1 to 4 are highly similar, the test results are illustrated using the microscopic morphology of Example 2 as an example.
[0079] Figure 2 and Figure 3 The microscopic morphology of the surface and cross-section of the photothermal electrolyte membrane prepared in Example 2 is that the surface of the photothermal electrolyte membrane is uniform and dense, without obvious bubbles and holes, providing a continuous transmission path for lithium ions and ensuring the rapid ion transmission of the photothermal electrolyte. The cross-sectional thickness of the photothermal electrolyte membrane is about 96 μm.
[0080] 2. Room temperature ionic conductivity test
[0081] In an Ar glove box, the photothermal electrolyte membranes prepared in Examples 1 to 4 and the electrolyte membrane prepared in Comparative Example 1 were cut into 10 mm discs and then placed between two pieces of stainless steel to form a sandwich structure as test samples.
[0082] The test samples were subjected to AC impedance testing in an electrochemical workstation with a frequency range of 1 MHz to 0.1 Hz from high frequency to low frequency to obtain the room temperature ionic conductivity of the test samples.
[0083] Test results such as Figure 4 As shown in FIG. 1 , the room temperature ionic conductivity of the electrolyte membrane of Comparative Example 1 is lower than that of Examples 1 to 4, that is, the lithiated poly(3,4-hydroxythiophene) can effectively improve the room temperature ionic conductivity of the electrolyte membrane; at the same time, Figure 4 It can be seen that when the mass ratio of PEO to lithiated poly(3,4-hydroxythiophene) reaches 100:5, the room temperature ionic conductivity performance of the prepared photothermal electrolyte membrane is the best, so the following tests are mainly based on Example 2.
[0084] 3. Electrochemical window test
[0085] In an Ar glove box, the photothermal electrolyte membrane prepared in Example 2 was cut into 10 mm discs and placed between stainless steel and lithium sheets to form a sandwich structure, and then a battery assembly test was carried out. Then, a linear sweep voltammetry (LSV) test was performed on the assembled battery using an electrochemical workstation, and the test potential range was 0 V to 6.55 V, and the scan rate was 1 m V / s.
[0086] The results are as follows Figure 5As shown, the electrochemical window of the photothermal electrolyte membrane prepared in Example 2 reaches above 5.3 V, indicating that the addition of lithiated poly(3,4-hydroxythiophene) in the electrolyte effectively improves the electrochemical window of the polymer electrolyte membrane, indicating that the photothermal electrolyte membrane prepared by the present invention meets the needs of most current commercial high-voltage positive electrode materials.
[0087] 4. Photothermal performance test
[0088] The photothermal electrolyte membrane prepared in Example 2 and the electrolyte membrane prepared in Comparative Example 1 were placed in a vacuum chamber at a power of 0.8 W cm -1 The samples were irradiated with 808 nm laser for 1 min.
[0089] The heating curves of Example 2 and Comparative Example 1 are as follows: Figure 6 As shown, the surface temperature of the photothermal electrolyte membrane prepared in Example 2 can quickly rise to above 140°C within 1 minute, while the surface temperature of Comparative Example 1 does not increase significantly within 1 minute, that is, there is no photothermal conversion effect, indicating that the addition of lithiated poly(3,4-hydroxythiophene) to the electrolyte in the present invention can enable the prepared electrolyte to have excellent photothermal conversion performance.
[0090] 5. Cycle performance test
[0091] In an Ar glove box, the photothermal electrolyte membrane prepared in Example 2 was cut into 16 mm discs, and then placed between two lithium sheets to form a sandwich structure to prepare a lithium symmetric battery.
[0092] Cyclic performance test was carried out in the Land test system with a current density of 0.1 mA cm -2 During the test, the charging and discharging process is alternated every half an hour.
[0093] The results are as follows Figure 7 As shown, the lithium symmetrical battery using the photothermal electrolyte membrane prepared in Example 2 can be stably cycled for more than 800 hours without short circuit, indicating that the photothermal electrolyte membrane prepared in the present invention has excellent cycle performance.
[0094] 6. Cyclic performance test of all-solid-state lithium metal battery
[0095] 6-1) The battery prepared in Example 5 was subjected to a cycle performance test at 45°C and a current density of 1C-2C.
[0096] 6-2) The batteries prepared in Example 6 and Comparative Example 2 were subjected to cycle performance tests at 45° C. and a current density of 0.2C.
[0097] Example 5 Test results are as follows Figure 8 As shown, from Figure 8It can be seen that the initial discharge capacity of Example 5 at 1C and 2C rates is 147.5 mAh g -1 and 118mAh g -1 The discharge capacity after 100 cycles is 138.5 mAh g -1 and 106.2mAh g -1 , the capacity retention rates were 93.9% and 90.0% respectively.
[0098] The test results of Example 6 and Comparative Example 2 are as follows Fig. 9 As shown, from Fig. 9 It can be seen that the initial discharge capacity of Example 6 at 0.2C rate is 160.7 mAh g -1 The discharge capacity after 100 cycles is 136.6 mAh g -1 The capacity retention rate is 85.0%, and the initial discharge capacity of comparative example 2 at 0.2C rate is 115.6 mAh g -1 The discharge capacity after 100 cycles is 93.5 mAh g -1 The capacity retention rate is 80.8%, which is lower than that of Example 6.
[0099] In summary, the photothermal electrolyte prepared by the present invention and the positive electrode material LiFePO4 or LiNi 0.5 Co 0.2 Mn 0.3 O2 assembly can produce solid-state batteries with good cycle performance, demonstrating the good adaptability of the photothermal electrolyte of the present invention to different battery systems.
[0100] 7. Photothermal performance test under low temperature environment
[0101] Example 7 was placed in an ambient temperature of -5°C and irradiated under a xenon lamp light source for 5 minutes.
[0102] The temperature rise curve of Example 7 under xenon lamp irradiation is as follows Fig.10 As shown, the working temperature of Example 7 can be quickly increased to above 80° C. within 5 minutes, indicating that the present invention can operate in a sub-zero low temperature environment.
[0103] 8. Charge and discharge performance test under low temperature environment
[0104] Example 7 was placed in an ambient temperature of -5°C and irradiated under a xenon lamp light source for 5 minutes, and then the charge and discharge performance was tested at different current densities.
[0105] The charge and discharge curves of Example 7 under xenon lamp irradiation are as follows: Fig.11 As shown, the discharge specific capacities of Example 7 at 0.3, 0.5, 1, 2, and 4C rates are 136.1 mAh g-1 、131.3mAh g -1 , 118.3mAh g -1 , 99.9mAh g -1 and 65.3mAh g -1 , indicating that Example 7 can achieve fast charging cycle in a sub-zero low temperature environment without additional power loss.
[0106] The above examples and comparative examples, based on the performance comparison of whether or not lithiated poly(3,4-hydroxythiophene) is contained, demonstrate the effectiveness of the present invention in improving the electrical properties of PEO-based polymer electrolytes and the low-temperature application potential of the photothermal conversion effect in solid-state lithium batteries.
[0107] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also change and modify the above implementation modes. Therefore, the present invention is not limited to the specific implementation modes disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A photothermal electrolyte, It is characterized in that The preparation raw materials include polyethylene oxide, lithium salt and filler; The filler is lithiated poly(3,4-hydroxythiophene).
2. The photothermal electrolyte according to claim 1, It is characterized in that The mass ratio of the polyethylene oxide, the lithium salt and the lithiated poly(3,4-hydroxythiophene) is 100:60:2.5-10; The lithium salt is lithium bis(trifluoromethanesulfonyl)imide.
3. A method for preparing a photothermal electrolyte, It is characterized in that The steps include: 1) In an inert gas atmosphere, polyethylene oxide, lithium salt and lithiated poly(3,4-hydroxythiophene) are placed in an organic solvent and mixed uniformly; 2) The solution prepared in step 1) is spread out and then dried to form a film, thereby obtaining a film-like photothermal electrolyte.
4. The method for preparing the photothermal electrolyte according to claim 3, It is characterized in that In step 1), the inert gas is argon, and the organic solvent is anhydrous acetonitrile; The drying operation of step 2) is specifically as follows: firstly naturally dry to form a film, and then place it in a vacuum environment at 55-65° C. to continue drying until the residual organic solvent is removed.
5. Use of the photothermal electrolyte according to any one of claims 1 to 4 in a solid-state battery.
6. A photothermal all-solid-state lithium metal battery, It is characterized in that Includes the photothermal electrolyte described in claims 1 and 2.
7. The photothermal all-solid-state lithium metal battery according to claim 6, It is characterized in that The photothermal all-solid-state lithium metal battery is stacked with a lithium metal negative electrode sheet, the photothermal electrolyte, a positive electrode sheet and the photothermal electrolyte in sequence from bottom to top; The thickness of the photothermal electrolyte is 90-100 μm.
8. The photothermal all-solid-state lithium metal battery according to claim 6 or 7, It is characterized in that The method for preparing the positive electrode sheet comprises the following steps: S1. Weigh the positive electrode material, polyvinylidene fluoride and carbon black conductor in a mass ratio of 7.5-8.5:0.5-1.5:0.5-1.5, grind and mix; S2, adding an appropriate amount of solvent to the mixture ground in S1, and continuing to grind until a uniform electrode slurry is formed; S3, evenly coating the electrode slurry in S2 on the carbon-coated aluminum foil to form a uniform electrode coating, and performing vacuum drying at a temperature of 60 to 80° C. for 12 to 24 hours; S4, punching the sheet material dried in S3 to make the positive electrode sheet.
9. The photothermal all-solid-state lithium metal battery according to claim 8, It is characterized in that The positive electrode material is LiFePO4 or LiNi 0.5 Co 0.2 Mn 0.3 O 2 .
10. A solar thermal all-solid-state lithium metal battery that can operate at sub-zero temperatures. It is characterized in that A photothermal all-solid-state lithium metal battery comprising any one of claims 6 to 9; The photothermal all-solid-state lithium metal battery adopts transparent packaging.