High-light-transmittance electromagnetic shielding film and preparation method thereof
By adopting a high-transmittance structure and a high-power pulse magnetron sputtering process in the electromagnetic shielding film, the problem of low transmittance in the existing electromagnetic shielding film is solved, and high transmittance and resistance under low square resistance are achieved The environmental performance meets the needs of wireless charging modules and other scenarios.
Patent Information
- Application Number
- CN202410975094.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-29
AI Technical Summary
The existing electromagnetic shielding film has a low transmittance when it reaches low square resistance, which cannot meet the process requirements of specific application scenarios, especially in wireless charging module scenarios.
Adopt a high-transmittance electromagnetic shielding film structure, including a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index enhancement layer, a second protective layer and a capping layer, and a high-power pulse magnetron sputtering power supply The metal shielding layer is prepared by sputtering, and the layer structure is optimized based on the optical matching principle to improve transmittance.
It significantly improves the transmittance and environmental resistance of the shielding film, meets the needs of low square resistance and high transmittance, and is suitable for specific application scenarios.
Smart Images

Figure CN119053141A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electromagnetic shielding films, and in particular to a high-transmittance electromagnetic shielding film and a preparation method thereof. Background Art
[0002] The shielding principle of electromagnetic shielding film (EMI film) is mainly based on the characteristics of conductive and magnetic materials, and the shielding effect of electromagnetic radiation is achieved by reflecting, absorbing and attenuating electromagnetic waves. First, the electromagnetic shielding film uses the metal film layer on its surface to reflect electromagnetic waves to achieve the shielding effect. Secondly, the electromagnetic shielding film further achieves the shielding effect by absorbing the energy of electromagnetic waves.
[0003] At present, in the wireless charging module scenarios on some specific mobile phones and wearable devices, electromagnetic shielding films are required to ensure high transmittance while having low square resistance. For example, in the wireless charging modules commonly used in Apple products, the electromagnetic shielding films used in the die-cutting process and subsequent product processing, due to the recognition characteristics of the optical sensors on the production line, the electromagnetic shielding films used must have a transmittance of more than 30% in visible light when the square resistance is required to be 1 ohm to meet the process requirements. However, due to the matching problem between the film layers, the electromagnetic shielding film structure in the prior art has a relatively low transmittance when achieving low square resistance, which cannot meet the process requirements of back-end applications. Summary of the invention
[0004] The purpose of the present application is to provide a high-transmittance electromagnetic shielding film and a preparation method thereof, so as to solve the problem that the electromagnetic shielding film structure in the prior art has a relatively low transmittance when achieving low square resistance due to the matching problem between its film layers, and cannot meet the process requirements of back-end applications.
[0005] To achieve the above-mentioned object, the first aspect of the present application provides a high-transmittance electromagnetic shielding film, comprising a transparent substrate layer, a first protective layer, a metal shielding layer, a high-refractive index anti-reflection layer, a second protective layer and a capping layer stacked in sequence;
[0006] The refractive index of the high refractive index anti-reflection layer is greater than 1.68, the thickness of the high refractive index anti-reflection layer is 2-30 nm, the material of the first protective layer is a metal oxide with high transmittance, and the material of the second protective layer is a metal.
[0007] In one or more embodiments, the material of the high refractive index anti-reflection layer is one or more combinations of zinc aluminum oxide, titanium oxide, aluminum oxide, zinc oxide and indium tin oxide.
[0008] In one or more embodiments, the high refractive index anti-reflection layer is an organic coating.
[0009] In one or more embodiments, the transparent substrate layer is made of PET, PP, PE, PI or PC, and the thickness of the transparent substrate layer is 4 to 50 μm.
[0010] In one or more embodiments, the material of the first protective layer is one or a combination of zinc aluminum oxide, titanium oxide, niobium oxide, aluminum oxide and silicon oxide, and the thickness of the first protective layer is 2 to 30 nm.
[0011] In one or more embodiments, the material of the metal shielding layer is one or more combinations of gold, silver, copper, titanium, aluminum, palladium and platinum, and the thickness of the metal shielding layer is 5 to 60 nm.
[0012] In one or more embodiments, the material of the second protective layer is one or more combinations of nickel, chromium, titanium and zirconium, and the thickness of the second protective layer is 0.5-10 nm.
[0013] In one or more embodiments, the material of the capping layer is one or more combinations of titanium oxide, niobium pentoxide, silicon dioxide and zirconium oxide, and the thickness of the capping layer is 3 to 20 nm.
[0014] In one or more embodiments, the metal shielding layer is sputtered using a high-power pulsed magnetron sputtering power supply process.
[0015] To achieve the above object, the second aspect of the present application provides a method for preparing a high-transmittance electromagnetic shielding film according to any one of the above embodiments, comprising:
[0016] Preparing a first protective layer on the surface of the transparent substrate layer;
[0017] The metal shielding layer is prepared by sputtering metal on the surface of the first protective layer using a high-power pulsed magnetron sputtering power supply process;
[0018] Prepare the high refractive index anti-reflection layer on the surface of the metal shielding layer;
[0019] Preparing a second protective layer on the surface of the high refractive index anti-reflection layer;
[0020] A capping layer is prepared on the surface of the second protective layer.
[0021] Different from the prior art, the beneficial effects of this application are:
[0022] The high-transmittance electromagnetic shielding film of the present application is provided with a high-refractive-index anti-reflection layer on the surface of the metal shielding layer, which can enhance the environmental resistance and anti-reflection performance of the shielding film on the one hand, and improve the transmittance of the film on the other hand by utilizing the optical matching principle, thereby achieving low square resistance while ensuring high transmittance, which can meet the needs of specific application scenarios;
[0023] The preparation method of the present application adopts a high-power pulsed magnetron sputtering power supply process to sputter and prepare a metal shielding layer, which can improve the density of the metal shielding layer and reduce the thickness of the metal shielding layer, thereby further improving the permeability of the high-transmittance electromagnetic shielding film. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art description are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 This is a schematic structural diagram of an embodiment of a high-transmittance electromagnetic shielding film of the present application;
[0026] Figure 2 It is a schematic flow chart of an embodiment of a method for preparing a high-transmittance electromagnetic shielding film of the present application;
[0027] Figure 3 This is a scanning electron microscope image of Effect Example 2 of the present application.
[0028] As shown in the figure:
[0029] A transparent substrate layer 100;
[0030] A first protective layer 200;
[0031] Metal shielding layer 300;
[0032] High refractive index anti-reflection layer 400;
[0033] A second protective layer 500;
[0034] Capping layer 600 . DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solutions in the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work should fall within the scope of protection of this application.
[0036] At present, portable electronic devices usually use electromagnetic shielding film structures with magnetron sputtering nano-scale shielding layers on polymer substrates. Its lightweight and easy-to-bend characteristics can meet the electromagnetic shielding function requirements of most electronic devices. However, when used in wireless charging module scenarios on certain specific mobile phones and wearable devices, the transmittance of the electromagnetic shielding film used cannot meet the process requirements of the product. For example, the electromagnetic shielding film used in the wireless charging module commonly used by Apple products has a transmittance of more than 30% in visible light to meet the process requirements when the square resistance of the electromagnetic shielding film used is required to be 1 ohm due to the recognition characteristics of the optical sensor of the production line during the die-cutting process and subsequent product processing. The conventional structure of the electromagnetic shielding film structure has a relatively low transmittance when the square resistance is low due to the matching problem between the film layers, which cannot meet the process requirements of the back-end application.
[0037] In order to solve the above problems, the applicant has developed a new type of high-transmittance electromagnetic shielding film, which can, on the one hand, enhance the environmental resistance and anti-reflection performance of the shielding film, and on the other hand, can also utilize the optical matching principle to improve the transmittance of the film, thereby achieving low square resistance while ensuring high transmittance to meet the needs of specific application scenarios.
[0038] Specifically, see Figure 1 , Figure 1 It is a schematic structural diagram of an embodiment of a high-transmittance electromagnetic shielding film of the present application.
[0039] like Figure 1 As shown, the high-transmittance electromagnetic shielding film includes a transparent substrate layer, a first protective layer, a metal shielding layer, a high-refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0040] In one embodiment, the transparent substrate layer may be made of materials such as polyester (PET), polypropylene (PP), polyethylene (PE), polyimide (PI), polycarbonate (PC), etc., and its thickness may be 4 to 50 μm.
[0041] The metal shielding layer is used to achieve the electromagnetic shielding performance of the film. In one embodiment, the metal shielding layer can be made of metal elements with good conductivity such as gold, silver, copper, titanium, aluminum, palladium, platinum, or alloys of the above metals.
[0042] In one embodiment, the thickness of the metal shielding layer may be 5 to 60 nm. It should be understood that the thickness of the metal shielding layer is designed to meet the electromagnetic shielding requirements of the application scenario, and it can be adjusted based on the requirements of the shielding performance. In other embodiments, for specific application scenarios, the thickness of the metal shielding layer may not be 5 to 60 nm.
[0043] The refractive index of the high refractive index anti-reflection layer is greater than 1.68, and the thickness is 2 to 30 nm, so as to improve the transmittance of the film based on the optical matching principle, so that the shielding film can have a low square resistance while ensuring a high transmittance. At the same time, the high refractive index anti-reflection layer can also block water vapor, etc., and play a role in protecting the metal functional layer.
[0044] In one embodiment, the high refractive index anti-reflection layer may be made of metal oxide materials with a high refractive index, such as zinc aluminum oxide, titanium oxide, aluminum oxide, zinc oxide, and indium tin oxide.
[0045] In another embodiment, the high refractive index anti-reflection layer may also be an organic coating with a refractive index that meets the requirements, and the effect of this embodiment can be achieved. Exemplarily, the high refractive index anti-reflection layer may be an acrylic resin with high refractive index particles, such as Toyokomei TYZ70-RA01-CN, etc., or may be other types of resins that meet the refractive index requirements and thickness requirements, and the effect of this embodiment can be achieved.
[0046] Preferably, the high refractive index anti-reflection layer can be made of metal oxide. Since metal oxide is an electrolyte and its dielectric constant and refractive index are different from those of the metal shielding layer, when the metal shielding layer is electroplated with a metal oxide nanocoating, the original optical response will be changed, thereby improving the anti-reflection properties of the metal film and allowing more light to penetrate the metal layer without being strongly reflected, thereby further improving the transmittance of the film.
[0047] In order to prevent the performance of the metal shielding layer from being affected by the external environment, in this embodiment, a first protective layer is further arranged between the transparent substrate layer and the metal shielding layer.
[0048] Among them, the material of the first protective layer can be a metal oxide with high transmittance such as zinc oxide, titanium oxide, niobium oxide, aluminum oxide, and silicon oxide, or a combination of the above materials, which can effectively block water vapor penetrating from the bottom of the transparent substrate layer, thereby improving the environmental resistance of the film.
[0049] In one embodiment, the thickness of the first protective layer may be 2-30 nm.
[0050] Furthermore, in order to prevent the performance of the metal shielding layer from being affected by the external environment, in this embodiment, the high-transmittance electromagnetic shielding film further includes a second protective layer arranged on a side of the high-refractive index anti-reflection layer away from the metal shielding layer.
[0051] The second protective layer is used to prevent oxidation and corrosion of the metal shielding layer by water, oxygen, acid, alkali, etc. In one embodiment, the second protective layer can be made of metal materials such as nickel, chromium, titanium, zirconium, and alloys of the above metals.
[0052] In one embodiment, the thickness of the second protective layer may be 0.5-10 nm.
[0053] In order to facilitate the laser cutting process of the shielding film and further improve the environmental resistance of the shielding film, in this embodiment, a capping layer may be arranged on the side of the second protective layer away from the high refractive index anti-reflection layer.
[0054] In one embodiment, the capping layer may be made of titanium oxide, niobium pentoxide, silicon dioxide, zirconium oxide, etc., and its thickness may be 3 to 20 nm.
[0055] The high-transmittance electromagnetic shielding film based on the above-mentioned embodiments can significantly improve the transmittance of the shielding film while ensuring the lower square resistance of the high-transmittance electromagnetic shielding film through thickness adjustment of each layer and material selection based on the optical matching principle, so that the electromagnetic shielding film can meet the process requirements of back-end applications in some application scenarios.
[0056] The present application also provides a method for preparing the high-transmittance electromagnetic shielding film of the above embodiment, please refer to Figure 2 , Figure 2 It is a schematic flow chart of an embodiment of a method for preparing a high-transmittance electromagnetic shielding film of the present application.
[0057] like Figure 2 As shown, the preparation method comprises:
[0058] S100, preparing a first protective layer on the surface of the transparent substrate layer.
[0059] Specifically, the preparation method of the first protective layer made of metal oxide material can be magnetron sputtering, and the raw materials and parameters of the magnetron sputtering can be the same as the magnetron sputtering method of the metal oxide film in the prior art.
[0060] For example, a metal may be used as a target material, and sputtering may be performed in an oxygen atmosphere at a power of 3 to 10 kW to obtain the first protective layer.
[0061] S200, sputtering metal on the surface of the first protective layer using a high-power pulsed magnetron sputtering power supply process to prepare a metal shielding layer.
[0062] The metal shielding layer is sputtered by a high-power pulsed magnetron sputtering power supply process. The process uses a high-power pulsed magnetron sputtering power supply as a power supply device, thereby depositing high-quality thin film materials in a pulsed manner under vacuum conditions.
[0063] High-power pulsed magnetron sputtering power supplies have a high ionization rate and can produce extremely high-density plasma, so that the sputtered atoms or molecules have a higher ionization rate, which helps to form a denser and more adherent film.
[0064] In addition, due to the pulse characteristics of the high-power pulsed magnetron sputtering power supply, a large amount of energy can be injected in a short time, and then the particles are allowed to rearrange and adsorb in the low-energy stage, thereby improving the microstructure and interface properties of the film, so that the film usually has excellent crystalline quality and chemical purity.
[0065] The metal shielding layer sputtered based on the high-power pulsed magnetron sputtering power supply process can significantly reduce its thickness while protecting the shielding requirements, thereby further improving the transmittance of the shielding film.
[0066] In one embodiment, the power of the high-power pulsed magnetron sputtering power supply may be 1-10 kW, the target material may be metal, and magnetron sputtering is performed in an argon atmosphere to obtain a metal shielding layer.
[0067] S300, preparing a high refractive index anti-reflection layer on the surface of the metal shielding layer.
[0068] In one embodiment, when the material of the high refractive index anti-reflection layer is metal oxide, its preparation method may be magnetron sputtering, and the raw materials and parameters of the magnetron sputtering may be the same as the magnetron sputtering method of the metal oxide film in the prior art.
[0069] For example, a metal may be used as a target material and sputtered at a power of 3 to 10 kW in an oxygen atmosphere to obtain a high refractive index anti-reflection layer.
[0070] In another embodiment, when the high refractive index anti-reflection layer is an organic resin with a refractive index that meets the requirements, the high refractive index anti-reflection layer can also be obtained by coating the resin and curing it.
[0071] S400, preparing a second protective layer on the surface of the high refractive index anti-reflection layer.
[0072] The second protective layer made of metal can be prepared by magnetron sputtering, and the raw materials and parameters of the magnetron sputtering can be the same as the magnetron sputtering method of the metal film in the prior art.
[0073] For example, a metal may be used as a target material, and sputtering may be performed in an argon atmosphere at a power of 3 to 10 kW to obtain the second protective layer.
[0074] S500, preparing a capping layer on the surface of the second protective layer.
[0075] The capping layer made of metal oxide material can be prepared by magnetron sputtering, and the raw materials and parameters of the magnetron sputtering can be the same as the magnetron sputtering method of the metal oxide film in the prior art.
[0076] For example, a metal may be used as a target material and sputtered in an oxygen atmosphere at a power of 0.5 to 5 kW to obtain a capping layer.
[0077] Based on the above preparation method, the metal shielding layer is prepared by sputtering using a high-power pulsed magnetron sputtering power supply process, which can significantly improve the density of the metal shielding layer and greatly reduce the thickness of the metal shielding layer, thereby further improving the permeability of the electromagnetic shielding film.
[0078] The technical effects of the technical solution of the present application are further elaborated in detail below in conjunction with specific embodiments.
[0079] Embodiment 1:
[0080] A metal film adopts a PET substrate, and magnetron sputters metal silver on the surface of the substrate by using a high-power pulsed magnetron sputtering power supply process, with a thickness of about 10nm.
[0081] Comparative Example 1:
[0082] A metal film is prepared by using the same PET substrate as in Example 1, and magnetron sputtering metal silver on the surface of the substrate using a conventional DC power supply, with a thickness of about 10 nm.
[0083] Effect example 1:
[0084] The square resistance of the metal films of Example 1 and Comparative Example 1 was measured by a square resistance measuring instrument using a probe measurement method; the transmittance of the metal films of Example 1 and Comparative Example 1 for visible light of 380-780 nm was measured by a transmittance detector, and the data in the following table were obtained.
[0085] Membrane structure Square resistance Transmittance (380nm-780nm) Example 1 2.4Ω / □ 74% Comparative Example 1 3.8Ω / □ 80%
[0086] Based on the above experimental data, it can be seen that under the premise of the same metal film thickness, the square resistance of the metal film sputtered by a high-power pulsed magnetron sputtering power supply is much lower than that of the metal film sputtered by a conventional DC power supply. This shows that the density of the metal film can be improved by the high-power pulsed magnetron sputtering power supply process.
[0087] In addition, under the premise that the thickness of the metal film is the same, the transmittance of the metal film of Example 1 is lower than that of the metal film of Comparative Example 1. This is mainly because the density of the metal film of Example 1 is higher than that of Comparative Example 1.
[0088] It can be understood that when a metal film is prepared by sputtering using the same amount of metal raw material, the thickness of the metal film using a high-power pulsed magnetron sputtering power supply can be significantly lower than that of the metal film using a DC power supply, and the transmittance can be higher than that of the metal film using a DC power supply.
[0089] Effect Example 2:
[0090] The metal films of Example 1 and Comparative Example 1 were subjected to cross-sectional characterization analysis to obtain Figure 3 , Figure 3 This is a scanning electron microscope image of Effect Example 2 of the present application.
[0091] like Figure 3 As shown, the density and interface smoothness of the metal film of Example 1 are significantly higher than those of Comparative Example 1. It can be seen that the metal film prepared by sputtering using a high-power pulsed magnetron sputtering power supply has better density and interface smoothness than the metal film sputtered by conventional DC direct current, which helps to reduce the thickness of the metal film and improve its permeability.
[0092] Embodiment 2:
[0093] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0094] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 20nm thick zinc oxide aluminum layer, the metal shielding layer is a 25nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 20nm thick zinc oxide aluminum layer, the second protective layer is a 1nm thick nickel-chromium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0095] Embodiment 3:
[0096] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0097] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 10nm thick silicon oxide layer, the metal shielding layer is a 25nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 20nm thick zinc oxide aluminum layer, the second protective layer is a 1nm thick nickel-chromium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0098] Embodiment 4:
[0099] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0100] Among them, the transparent substrate layer is a PP layer with a thickness of 50μm, the first protective layer is a 10nm thick titanium oxide layer, the metal shielding layer is a 40nm thick metal copper layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 2nm thick titanium oxide layer, the second protective layer is a 10nm thick nickel layer, and the capping layer is a 3nm thick silicon dioxide layer.
[0101] Embodiment 5:
[0102] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0103] Among them, the transparent substrate layer is a PE layer with a thickness of 10μm, the first protective layer is a 2nm thick niobium oxide layer, the metal shielding layer is a 10nm thick metal platinum layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 30nm thick indium tin oxide layer, the second protective layer is a 0.5nm thick titanium layer, and the capping layer is a 20nm thick titanium oxide layer.
[0104] Embodiment 6:
[0105] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0106] Among them, the transparent substrate layer is a PI layer with a thickness of 30μm, the first protective layer is a 3nm thick zinc oxide aluminum layer, the metal shielding layer is a 60nm thick metal titanium layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 15nm thick zinc oxide layer, the second protective layer is a 5nm thick zirconium layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0107] Embodiment 7:
[0108] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0109] Among them, the transparent substrate layer is a PET layer with a thickness of 4μm, the first protective layer is a 30nm thick aluminum oxide layer, the metal shielding layer is a 10nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 15nm thick zinc oxide layer, the second protective layer is a 5nm thick nickel-titanium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0110] Embodiment 8:
[0111] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0112] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 15nm thick titanium oxide layer, the metal shielding layer is a 10nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the high refractive index anti-reflection layer is a 15nm thick acrylic resin layer, model Toyo Kemei TYZ70-RA01-CN, the second protective layer is a 5nm thick nickel-titanium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0113] Comparative Example 2:
[0114] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0115] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 20nm thick zinc oxide aluminum layer, the metal shielding layer is a 40nm thick metal silver layer obtained by sputtering using a DC power supply, the high refractive index anti-reflection layer is a 20nm thick zinc oxide aluminum layer, the second protective layer is a 1nm thick nickel-chromium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0116] Comparative Example 3:
[0117] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a second protective layer and a capping layer which are stacked in sequence.
[0118] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a zinc oxide aluminum layer with a thickness of 20nm, the metal shielding layer is a 25nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the second protective layer is a nickel-chromium alloy layer with a thickness of 1nm, and the capping layer is a 10nm thick niobium pentoxide layer.
[0119] Comparative Example 4:
[0120] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence.
[0121] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 10nm thick silicon oxide layer, the metal shielding layer is a 40nm thick metal silver layer obtained by sputtering using a DC power supply, the high refractive index anti-reflection layer is a 20nm thick zinc oxide aluminum layer, the second protective layer is a 1nm thick nickel-chromium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0122] Comparative Example 5:
[0123] An electromagnetic shielding film comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a second protective layer and a capping layer which are stacked in sequence.
[0124] Among them, the transparent substrate layer is a PET layer with a thickness of 20μm, the first protective layer is a 10nm thick silicon oxide layer, the metal shielding layer is a 25nm thick metal silver layer sputtered by a high-power pulsed magnetron sputtering power supply, the second protective layer is a 1nm thick nickel-chromium alloy layer, and the capping layer is a 10nm thick niobium pentoxide layer.
[0125] Effect example 3:
[0126] The square resistance of the electromagnetic shielding films of Examples 2, 3 and Comparative Examples 2 to 4 was measured with a square resistance measuring instrument using a probe measurement method; the transmittance of the electromagnetic shielding films of Examples 2, 3 and Comparative Examples 2 to 4 for visible light of 380-780 nm was measured with a transmittance detector to obtain the data in the following table.
[0127] Membrane structure Square resistance Transmittance (380nm-780nm) Example 2 1Ω / □ 35% Example 3 1Ω / □ 31% Comparative Example 2 1Ω / □ 17% Comparative Example 3 1Ω / □ 24% Comparative Example 4 1Ω / □ 14% Comparative Example 5 1Ω / □ 20%
[0128] Based on the data in the above table, it can be seen that the square resistance of Examples 2, 3 and Comparative Examples 2 to 4 is relatively low, reaching 1Ω / □, but the transmittance of Comparative Examples 2 to 5 is much lower than that of Examples 2 and 3.
[0129] Specifically, comparing the data of Example 2 and Comparative Example 2, the difference between Comparative Example 2 and Example 2 is that the metal shielding layer of Example 2 is sputtered by a high-power pulsed magnetron sputtering power supply, the metal shielding layer has a high density and a thickness of 25nm, while the metal shielding layer of Comparative Example 2 is sputtered by a DC direct current power supply, and the thickness of the metal shielding layer is 40nm. The transmittance of Example 2 is increased by 106% over that of Comparative Example 2.
[0130] Comparing the data of Example 3 and Comparative Example 4, the difference between Comparative Example 4 and Example 3 is that the metal shielding layer of Example 3 is sputtered by a high-power pulsed magnetron sputtering power supply, and the density of the metal shielding layer is high, and the thickness is 25nm, while the metal shielding layer of Comparative Example 4 is sputtered by a DC direct current power supply, and the thickness of the metal shielding layer is 40nm. The transmittance of Example 3 is 121% higher than that of Comparative Example 4.
[0131] It can be seen from the above data that the use of high-power pulsed magnetron sputtering power supply to sputter and prepare the metal shielding layer can significantly reduce the thickness of the metal shielding layer and significantly improve the transmittance of the shielding film.
[0132] Comparing the data of Example 2 and Comparative Example 3, the difference between Comparative Example 3 and Example 2 is that Example 2 adds a 20nm thick zinc oxide aluminum layer as a high refractive index anti-reflection layer on the basis of Comparative Example 3. The square resistances of Example 2 and Comparative Example 3 both reach 1Ω / □. After adding the high refractive index anti-reflection layer, the square resistance of the shielding film remains at a low value. At the same time, the transmittance of Example 2 for 380-780nm visible light increases by 45.8% relative to Comparative Example 1, and the transmittance reaches 35%.
[0133] Comparing the data of Example 3 and Comparative Example 5, the difference between Comparative Example 5 and Example 3 is that Example 3 adds a 20 nm thick zinc oxide aluminum layer as a high refractive index anti-reflection layer on the basis of Comparative Example 5.
[0134] The square resistance of Example 3 and Comparative Example 5 both reach 1Ω / □. After adding a high refractive index anti-reflection layer, the square resistance of the shielding film remains at a low value. At the same time, the transmittance of 380-780nm visible light in Example 3 increases by 55% compared with Comparative Example 5, and the transmittance reaches 31%.
[0135] From the above data, it can be seen that the high refractive index anti-reflection layer effectively improves the transmittance of the shielding film; the reason is that the newly added high refractive index anti-reflection layer cooperates with other layers to improve the transmittance of the film based on the optical matching principle; at the same time, the zinc oxide aluminum layer is an electrolyte, and the dielectric constant and refractive index are different from the metal shielding layer. After adding the zinc oxide aluminum layer, the original optical response is changed, the anti-reflection performance of the metal film is improved, and more light penetrates the metal layer without being strongly reflected, thereby further improving the transmittance of the film.
[0136] In addition, by comparing the data of Example 2, Comparative Example 2 and Comparative Example 3, it can be seen that when the sputtering process of the metal shielding layer in the scheme of Example 2 is changed (Comparative Example 2), and when the high refractive index anti-reflection layer is cancelled (Comparative Example 3), excellent visible light transmittance cannot be achieved. Only using a high-power pulsed magnetron sputtering power supply process to sputter the metal shielding layer, but not adding a high refractive index anti-reflection layer, it is impossible to achieve excellent visible light transmittance; only adding a high refractive index anti-reflection layer, but using a conventional DC direct current power supply process to sputter the metal shielding layer, it is also impossible to achieve excellent visible light transmittance.
[0137] Therefore, it can be seen that in the solution of Example 2, the high-power pulsed magnetron sputtering power supply process of the metal shielding layer and the addition of the high refractive index anti-reflection layer have a synergistic effect, producing unexpected technical effects. Further, the same conclusion can be drawn by comparing the data of Example 3, Comparative Example 4 and Comparative Example 5.
[0138] For those skilled in the art, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
[0139] The foregoing description of the specific exemplary embodiments of the present application is for the purpose of illustration and illustration. These descriptions are not intended to limit the present application to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present application and its practical application, so that those skilled in the art can realize and utilize the various exemplary embodiments of the present application and various selections and changes. The scope of the present application is intended to be limited by the claims and their equivalents.
Claims
1. A high light transmittance electromagnetic shielding film, characterized in that: It comprises a transparent substrate layer, a first protective layer, a metal shielding layer, a high refractive index anti-reflection layer, a second protective layer and a capping layer which are stacked in sequence; The refractive index of the high refractive index anti-reflection layer is greater than 1.68, the thickness of the high refractive index anti-reflection layer is 2-30 nm, the material of the first protective layer is a metal oxide with high transmittance, and the material of the second protective layer is a metal.
2. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The material of the high refractive index anti-reflection layer is one or a combination of zinc aluminum oxide, titanium oxide, aluminum oxide, zinc oxide and indium tin oxide.
3. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The high refractive index anti-reflection layer is an organic coating.
4. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The material of the transparent substrate layer is PET, PP, PE, PI or PC, and the thickness of the transparent substrate layer is 4-50 μm.
5. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The material of the first protective layer is one or a combination of zinc aluminum oxide, titanium oxide, niobium oxide, aluminum oxide and silicon oxide, and the thickness of the first protective layer is 2-30 nm.
6. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The material of the metal shielding layer is one or more combinations of gold, silver, copper, titanium, aluminum, palladium and platinum, and the thickness of the metal shielding layer is 5-60nm.
7. The high light transmittance electromagnetic shielding film according to claim 1, characterized in that: The material of the second protective layer is one or more combinations of nickel, chromium, titanium and zirconium, and the thickness of the second protective layer is 0.5-10 nm.
8. The high light transmittance electromagnetic shielding film according to claim 7, characterized in that: The material of the capping layer is one or more combinations of titanium oxide, niobium pentoxide, silicon dioxide and zirconium oxide, and the thickness of the capping layer is 3-20 nm.
9. The high-transmittance electromagnetic shielding film according to any one of claims 1 to 8, characterized in that: The metal shielding layer is sputtered by using a high-power pulse magnetron sputtering power supply process.
10. A method for preparing a high-transmittance electromagnetic shielding film according to any one of claims 1 to 9, characterized in that: include: Preparing the first protective layer on the surface of the transparent substrate layer; The metal shielding layer is prepared by sputtering metal on the surface of the first protective layer using a high-power pulsed magnetron sputtering power supply process; Prepare the high refractive index anti-reflection layer on the surface of the metal shielding layer; Prepare the second protective layer on the surface of the high refractive index anti-reflection layer; The capping layer is prepared on the surface of the second protective layer.