Mesoscopic perovskite solar cell based on chiral perovskite heterojunction and preparation method thereof
By introducing chiral perovskite heterojunction structure into carbon-based perovskite solar cells, the interface contact between perovskite and carbon electrode is improved, the problem of hole diffusion and energy band mismatch is solved, and the energy conversion efficiency is improved and open circuit voltage and enhance device stability.
Patent Information
- Application Number
- CN202411171415.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
Carbon-based perovskite solar cells have low performance in terms of energy conversion efficiency and open circuit voltage, mainly due to the long-distance diffusion of holes and the lack of electron blocking effect of the perovskite/carbon interface.
Using chiral perovskite heterojunction structure, the perovskite precursor solution is filled in the mesoporous membrane skeleton and post-treatment, using chiral amine molecules or organic solutions of chiral ammonium salts to improve perovskite and carbon The interface contact of the electrodes forms a two-dimensional/three-dimensional chiral perovskite heterojunction, improving the built-in electric field and interface quality of the perovskite.
The energy conversion efficiency and open circuit voltage of solar cells are significantly improved, and the thermal stability and commercial feasibility of the device are enhanced, and the energy conversion efficiency is improved and the initial efficiency is maintained after long storage.
Smart Images

Figure FT_1 
Figure FT_2 
Figure BDA0005009382990000031
Abstract
Description
Technical Field
[0001] The present invention relates to the field of perovskite solar cells, and in particular to a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction and a preparation method thereof. Background Art
[0002] Carbon-based perovskite solar cells have attracted much attention due to their low-cost materials, excellent long-term stability and simple manufacturing process, and have broad application prospects. Mesoscopic perovskite solar cells (p-MPSCs) based on prefabricated triple mesoscopic layers (mesoporous TiO2 / mesoporous ZrO2 / mesoporous carbon electrode) are more advantageous in terms of cost and stability. In p-MPSCs, the mp-TiO2 layer is the electron transport layer, the porous carbon is the back electrode and hole collector, and the mp-ZrO2 layer insulates the mp-TiO2 from the carbon electrode. In this structure, the perovskite can transport holes to the back electrode. In addition, p-MPSCs can be fully prepared in ambient air without the need for a harsh preparation environment, which can further reduce costs and improve commercial feasibility. Although p-MPSCs have the advantages of low cost and stability compared to other device structures, they still face some challenges, such as lower power conversion efficiency (PCE) and larger open circuit voltage (V OC ) loss. There are two key factors that contribute to these challenges. First, the photogenerated holes need to pass through ≈2μm thick mp-ZrO2 to reach the carbon electrode, and the long-distance diffusion of holes leads to significant charge recombination. Second, there is no electron blocking effect at the perovskite / carbon interface, and the mismatched band alignment slows down the extraction of holes from the carbon electrode. This results in low open circuit voltage and energy conversion efficiency of p-MPSCs. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction and a preparation method thereof, which can effectively improve the contact interface between the carbon electrode and the perovskite layer, reduce interface defects and interface impedance, and enhance the built-in electric field of the perovskite, thereby greatly improving the open circuit voltage and energy conversion efficiency of the device.
[0004] The technical solution adopted by the present invention is:
[0005] The present invention provides a method for preparing a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction, which comprises the following steps:
[0006] Taking a mesoporous membrane skeleton, filling it with a perovskite precursor solution, and after the perovskite is crystallized, filling the mesoporous membrane skeleton with a post-treatment solution and annealing to obtain the mesoscopic perovskite solar cell;
[0007] The post-treatment solution is an organic solution containing chiral amine molecules or chiral ammonium salts.
[0008] Preferably, the perovskite material structure is an ABX3 type organic-inorganic hybrid perovskite material, wherein A is one or more of methylamine cation, formamidinium cation, acetamidine cation, cesium ion, lithium ion, potassium ion, sodium ion, and rubidium ion, B is one or more of lead ion, tin ion, copper ion, germanium ion, manganese ion, ferrous ion, cobalt ion, nickel ion, zinc ion, and magnesium ion, and X is one or more of fluoride ion, chloride ion, bromide ion, iodide ion, boron tetrafluoride anion, and thiocyanate anion;
[0009] Preferably, the solvent used in the perovskite precursor solution is one or more of γ-butyrolactone, N,N-dimethylformamide, dimethyl sulfoxide, methanol, ethanol, isopropanol, methylamine, ethylamine, acetonitrile, triethylamine, and propylamine;
[0010] Preferably, the chiral amine molecule or chiral ammonium salt has the following general structure:
[0011]
[0012] Wherein, R1 and R3 are each independently selected from halogen-substituted or unsubstituted aryl, C5-C6 cycloalkyl, C3-C6 azacycloalkyl, C1-C6 alkyl, R2 is selected from C1-C3 alkylene or does not exist; X is selected from halogen.
[0013] Preferably, R1 is selected from C1-C3 alkyl, and R3 is selected from halogen-substituted or unsubstituted phenyl, naphthyl, anthracenyl, pyrenyl, C5-C6 cycloalkyl, C4-C5 azacycloalkyl, C1-C6 alkyl.
[0014] Preferably, the chiral amine molecule is one or more non-racemic compounds selected from (S)-methylbenzylamine or (R)-methylbenzylamine, (S)-methylphenethylamine or (R)-methylphenethylamine, (S)-4-chlorophenylethylamine or (R)-4-chlorophenylethylamine, (S)-naphthylethylamine or (R)-naphthylethylamine, (S)-cyclohexylethylamine or (R)-cyclohexylethylamine, (S)-3-aminopiperidine or (R)-3-aminopiperidine, (S)-2-aminooctane or (R)-2-aminooctane, and the chiral ammonium salt is the hydrochloride, hydrobromide, hydroiodide, tetrafluoroborate or thiocyanate corresponding to the above chiral amine molecules. The chemical structure of the above preferred compounds is as follows (stereostructure is not marked):
[0015]
[0016] Preferably, the solvent of the organic solution is one or more of methanol, ethanol, propanol, butanol, pentanol, isopropanol, isobutanol, isopentanol, toluene, chlorobenzene and chloroform.
[0017] Preferably, the solvent of the organic solution is one or more of methanol, ethanol, propanol, butanol, amyl alcohol, isopropanol, isobutanol, isopentanol, toluene, chlorobenzene, and chloroform;
[0018] Preferably, the structure of the mesoporous membrane skeleton including a conductive substrate, a mesoporous metal oxide, an insulating spacer layer and a carbon electrode is a mesoporous or planar structure; the mesoporous membrane skeleton is prepared by one or more of a scraping method or a printing method; the thickness of the dense metal oxide is 10-500nm; the thickness of the insulating spacer layer is 0.1-20μm; the thickness of the carbon electrode is 2-50μm; preferably, the filling of the perovskite precursor solution is by spontaneous diffusion into the mesoporous structure after at least one of drip coating, spraying, scraping and printing on the surface of the carbon electrode.
[0019] Preferably, the post-treatment solution is filled into the mesoporous membrane skeleton by at least one method selected from the group consisting of drip coating, spray coating, blade coating and printing after the perovskite precursor solution is crystallized.
[0020] Preferably, the annealing temperature of the perovskite precursor solution is 0-150° C., and the annealing time is 0-48 h; the annealing temperature of the post-treatment solution is 0-100° C., and the annealing time is 0-48 h.
[0021] Preferably, the chiral ammonium salt in the post-treatment solution reacts with PbI2 to form a two-dimensional chiral perovskite, or the chiral amine molecules in the post-treatment solution react with the formamidinium cations in the perovskite material and form larger cations, which then react with PbI2 to form a two-dimensional chiral perovskite, and the two-dimensional chiral perovskite forms a two-dimensional / three-dimensional chiral perovskite heterojunction with the three-dimensional perovskite.
[0022] Further preferably, the preparation method of the mesoscopic perovskite solar cell specifically includes the following steps: taking a porous membrane skeleton, filling it with a perovskite precursor solution, then annealing at 0-150°C to crystallize the perovskite, and then placing it at a temperature of 20-25°C and a relative humidity of 50-70% RH for post-treatment with a post-treatment solution, wherein the concentration of the post-treatment solution is 0-150 mg / ml, and the annealing time is 0-48h; by post-treating the porous membrane skeleton, a chiral halogen ammonium salt reacts with PbI2 to form a two-dimensional chiral perovskite, or a chiral amine molecule selectively reacts with a carboxamidinium cation in the perovskite material to form a larger amidine cation, and these cations subsequently react with PbI2 to form a two-dimensional chiral perovskite, and the two-dimensional chiral perovskite forms a chiral perovskite heterojunction with the three-dimensional perovskite.
[0023] The present invention further provides a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction, wherein the cell is prepared by the above method.
[0024] The beneficial effects of the present invention are:
[0025] The present invention uses chiral amine molecules or chiral ammonium salts dissolved in an organic solvent as a post-treatment solution to perform interface post-treatment on a porous carbon electrode, so that the post-treatment solution penetrates into the carbon electrode and contacts the perovskite material, and then the chiral ammonium salt in the post-treatment solution reacts with PbI2 to form a two-dimensional chiral perovskite, or the chiral amine molecules selectively react with cations in the perovskite material near the carbon electrode and form larger cations, which then react with PbI2 to form a two-dimensional chiral perovskite, and the two-dimensional chiral perovskite forms a chiral perovskite heterojunction with the three-dimensional perovskite. On the one hand, by introducing highly hydrophobic and large-sized organic cations, the three-dimensional perovskite can be cut down to obtain a low-dimensional perovskite material, which improves the humidity instability of the three-dimensional perovskite to a certain extent and enhances the thermal stability. On the other hand, by combining the organic-inorganic hybrid perovskite components with chirality, the introduction of chiral amine molecules can make the perovskite crystallize in a chiral space group and present chiral characteristics. The chiral two-dimensional perovskite breaks the spatial inversion symmetry of the perovskite crystal and establishes a chiral-ferroelectric heterojunction polarity system. High-voltage ferroelectric photovoltaic devices can be obtained by utilizing the residual polarization field effect of ferroelectric materials. At the same time, since a wide-bandgap two-dimensional perovskite interface layer material is constructed between the perovskite and the mesoporous electrode layer, the mismatch between the perovskite and the carbon electrode mesoporous electrode layer can be reduced, and the open circuit voltage of the device can be increased, thereby improving the device efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a JV curve graph of comparative example 1 (mesoscopic perovskite solar cell obtained without post-treatment with chiral amine molecules), comparative example 2 (chiral amine molecules added to the precursor solution), embodiment 1, embodiment 2, embodiment 3 and embodiment 4 (mesoscopic perovskite solar cell obtained after post-treatment with chiral amine molecules) of the present invention tested in air under unpackaged conditions.
[0027] Figure 2 1 and 2 are PCE curves of Comparative Example 1, Example 1, Example 2, Example 3 and Example 4 of the present invention. DETAILED DESCRIPTION
[0028] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work all fall within the scope of protection of the present invention.
[0029] Comparative Example 1:
[0030] This comparative example provides a mesoscopic perovskite solar cell without a chiral perovskite heterojunction, comprising the following steps:
[0031] (1) Preparation of mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of Cs was drop-coated on the top of the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 The perovskite precursor solution infiltrates and fills the mesoporous zirconia and mesoporous titanium dioxide from top to bottom from the mesoporous carbon electrode in sequence, and a mesoscopic perovskite solar cell is prepared after annealing at 60°C for 20 hours.
[0032] See also Figure 1 , Figure 2 The perovskite solar cell without a chiral perovskite heterojunction obtained in step (1) was subjected to a JV curve test, and the energy conversion efficiency of the solar cell was 17.51%; after being stored in air for 1500 hours, the PCE decreased to less than 80% of the initial efficiency.
[0033] Comparative Example 2:
[0034] This comparative example provides a mesoscopic perovskite solar cell containing chiral amine molecules in a perovskite precursor solution, comprising the following steps:
[0035] (1) Preparation of mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of 1 mol / L Cs containing 5% (S)-methylbenzylamine was drop-coated on the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 (1 mol / L) perovskite precursor solution was used to infiltrate and fill the mesoporous zirconia and mesoporous titania from top to bottom from the mesoporous carbon electrode. After annealing at 60°C for 20h, a mesoscopic perovskite solar cell was prepared.
[0036] See also Figure 1The JV curve test of the perovskite solar cell containing chiral amine molecules in the perovskite precursor liquid obtained in step (1) was performed, and the energy conversion efficiency of the solar cell was 12.59%.
[0037] Embodiment 1:
[0038] This embodiment provides a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction induced by (S)-methylbenzylamine and a preparation method thereof, comprising the following steps:
[0039] (1) Preparation of mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of Cs was drop-coated on the top of the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 The perovskite precursor solution infiltrates and fills the mesoporous zirconia and mesoporous titanium dioxide from top to bottom from the mesoporous carbon electrode in sequence, and a mesoscopic perovskite solar cell is prepared after annealing at 60°C for 20 hours.
[0040] (2) Post-treatment of chiral amine molecules or chiral ammonium halides: S-methylbenzylamine / isopropanol solution was coated on the carbon electrode, and then annealed at 25°C for 15 min to form a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction.
[0041] See also Figure 1 , Figure 2 In this embodiment, the mesoscopic perovskite solar cell based on the chiral perovskite heterojunction obtained by post-treatment of the (S)-methylbenzylamine / isopropanol solution interface was subjected to JV curve test, and its energy conversion efficiency was 19.46%. After being stored in air for 3000 hours, the PCE still maintained more than 95% of the initial efficiency. This shows that the chiral perovskite heterojunction induced by S-methylbenzylamine can improve the energy conversion efficiency and stability of the mesoscopic perovskite solar cell.
[0042] Embodiment 2:
[0043] This embodiment provides a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction induced by (S)-3-aminopiperidine and a preparation method thereof, comprising the following steps:
[0044] (1) Preparation of mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of Cs was drop-coated on the top of the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 The perovskite precursor solution infiltrates and fills the mesoporous zirconia and mesoporous titanium dioxide from top to bottom from the mesoporous carbon electrode in sequence, and a mesoscopic perovskite solar cell is prepared after annealing at 60°C for 20 hours.
[0045] (2) Interface post-treatment: (S)-3-aminopiperidine / isopropanol solution was coated on the carbon electrode, and then annealed at 70°C for 15 min to form a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction.
[0046] See also Figure 1 , Figure 2 In this embodiment, the solar cell obtained by post-treatment of the (S)-3-aminopiperidine / isopropanol solution interface was subjected to JV curve test, and its energy conversion efficiency was 19.70%. After being stored in air for 3000 hours, the PCE still maintained more than 95% of the initial efficiency. This shows that the chiral perovskite heterojunction induced by S-methylbenzylamine can improve the energy conversion efficiency and stability of mesoscopic perovskite solar cells.
[0047] Embodiment 3:
[0048] This embodiment provides a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction induced by (S)-naphthylethylamine and a preparation method thereof, comprising the following steps:
[0049] (1) Preparation of printed mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of Cs was drop-coated on the top of the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 The perovskite precursor solution infiltrates and fills the mesoporous zirconia and mesoporous titania from top to bottom from the mesoporous carbon electrode in sequence, and a printed mesoscopic perovskite solar cell is prepared after annealing at 60°C for 20 hours.
[0050] (2) Interface post-treatment: (S)-naphthylethylamine / isopropanol solution was coated on the carbon electrode, and then annealed at 70°C for 15 min to form a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction.
[0051] See also Figure 1 , Figure 2 In this embodiment, the mesoscopic perovskite solar cell based on the chiral perovskite heterojunction obtained by post-treatment of the (S)-naphthylethylamine / isopropanol solution interface was subjected to JV curve test, and its energy conversion efficiency was 20.06%. After being stored in air for 3000 hours, the PCE still maintained more than 95% of the initial efficiency. This shows that the chiral perovskite heterojunction induced by (S)-naphthylethylamine can improve the energy conversion efficiency of mesoscopic solar cells.
[0052] Embodiment 4:
[0053] This embodiment is based on a mesoscopic perovskite solar cell of a chiral perovskite heterojunction induced by (R)-2-aminooctane and a preparation method thereof, comprising the following steps:
[0054] (1) Preparation of mesoscopic perovskite solar cells: On a FTO glass substrate, a 40 nm thick dense titanium dioxide film was prepared by spray pyrolysis, a 600 nm thick mesoporous titanium dioxide layer was prepared by printing, a 2 μm thick mesoporous zirconium oxide layer was prepared by printing, and a 20 μm thick carbon electrode was prepared by printing carbon slurry. After sintering at 400 °C and cooling to room temperature, 5 μL of Cs was drop-coated on the mesoporous carbon electrode. 0.05 MA 0.15 FA 0.8 PbI3·MACl 0.2 The perovskite precursor solution infiltrates and fills the mesoporous zirconia and mesoporous titanium dioxide from top to bottom from the mesoporous carbon electrode in sequence, and a mesoscopic perovskite solar cell is prepared after annealing at 60°C for 20 hours.
[0055] (2) Interface post-treatment: A (R)-2-aminooctane / isopropanol solution was coated on the carbon electrode, and then annealed at 70°C for 15 min to form a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction after interface post-treatment.
[0056] See also Figure 1 , Figure 2 In this embodiment, the solar cell obtained by post-treatment of the (R)-2-aminooctane / isopropanol solution interface was subjected to JV curve test, and its energy conversion efficiency was 19.41%. After being stored in air for 1200 hours, the PCE did not decay. This shows that the chiral perovskite heterojunction induced by (R)-2-aminooctane can improve the energy conversion efficiency of solar cells.
Claims
1. A method for preparing a mesoscopic perovskite solar cell based on a chiral perovskite heterojunction, comprising the following steps: Taking a mesoporous membrane skeleton, filling it with a perovskite precursor solution, and after the perovskite is crystallized, filling the mesoporous membrane skeleton with a post-treatment solution and annealing to obtain the mesoscopic perovskite solar cell; The post-treatment solution is an organic solution containing chiral amine molecules or chiral ammonium salts.
2. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The perovskite material structure is an ABX3 type organic-inorganic hybrid perovskite material, wherein A is one or more of methylamine cation, formamidinium cation, acetamidine cation, cesium ion, lithium ion, potassium ion, sodium ion, and rubidium ion, B is one or more of lead ion, tin ion, copper ion, germanium ion, manganese ion, ferrous ion, cobalt ion, nickel ion, zinc ion, and magnesium ion, and X is one or more of fluoride ion, chloride ion, bromide ion, iodide ion, boron tetrafluoride anion, and thiocyanate anion.
3. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The solvent used in the perovskite precursor solution is one or more of γ-butyrolactone, N,N-dimethylformamide, dimethyl sulfoxide, methanol, ethanol, isopropanol, methylamine, ethylamine, acetonitrile, triethylamine, and propylamine.
4. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The chiral amine molecule or chiral ammonium salt has the following general structure: Wherein, R1 and R3 are independently selected from halogen-substituted or unsubstituted aryl, C5-C6 cycloalkyl, C3-C6 azacycloalkyl, C1-C6 alkyl, R2 is selected from C1-C3 alkylene or does not exist; X is selected from halogen; preferably, R1 is selected from C1-C3 alkyl, R3 is selected from halogen-substituted or unsubstituted phenyl, naphthyl, anthracenyl, pyrenyl, C5-C6 cycloalkyl, C4-C5 azacycloalkyl, C1-C6 alkyl; the most preferred chiral amine molecules are: (S)-methylbenzylamine or (R)-methylbenzylamine, (S) -methylphenethylamine or (R)-methylphenethylamine, (S)-4-chlorophenylethylamine or (R)-4-chlorophenylethylamine, (S)-naphthylethylamine or (R)-naphthylethylamine, (S)-cyclohexylethylamine or (R)-cyclohexylethylamine, (S)-3-aminopiperidine or (R)-3-aminopiperidine, (S)-2-aminooctane or (R)-2-aminooctane or multiple non-racemic compounds, and the halogen ammonium salt is one or more of the hydrochloride, hydrobromide, hydroiodide, tetrafluoroborate or thiocyanate corresponding to the above chiral amine molecules.
5. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The solvent of the organic solution is one or more of methanol, ethanol, propanol, butanol, amyl alcohol, isopropanol, isobutanol, isopentanol, toluene, chlorobenzene and chloroform.
6. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The mesoporous membrane skeleton comprises a mesoporous or planar structure of a conductive substrate, a dense metal oxide layer, a mesoporous metal oxide layer, an insulating spacer layer and a carbon electrode; the mesoporous membrane skeleton is prepared by one or more of a scraping method or a printing method; the thickness of the dense metal oxide layer is 1-200nm; the thickness of the mesoporous metal oxide layer is 10nm-10μm; the thickness of the insulating spacer layer is 0.1-20μm; and the thickness of the carbon electrode is 1-50μm.
7. The preparation method according to claim 1, characterized in that: The perovskite precursor solution is filled into the mesoporous structure by spontaneous diffusion after being dripped, sprayed, scraped, printed, or printed on the surface of the carbon electrode.
8. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The post-treatment solution is filled into the mesoporous membrane skeleton by at least one method selected from the group consisting of drip coating, spray coating, scraping coating, printing and printing after the perovskite precursor solution is crystallized.
9. The method for preparing a mesoscopic perovskite solar cell according to claim 1, characterized in that: The annealing temperature of the perovskite precursor solution is 0-150° C., and the annealing time is 0-48 hours; the annealing temperature of the post-treatment solution is 0-100° C., and the annealing time is 0-48 hours.
10. A mesoscopic perovskite solar cell based on a chiral perovskite heterojunction, wherein the cell is prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Trans-perovskite solar cell with gradient structure and preparation method thereof
CN122396148A
A gradient structure transversal perovskite solar cell and a preparation method thereof
CN122396148B