Method and system for extracting iron value from red mud

Through induction heating technology, the iron nanoparticles in red mud are converted into magnetite and separated by magnetic separator, which solves the problem of low iron recovery in red mud in the existing technology, and achieves efficient and stable iron value recovery and Magnetite production.

CN119053714APending Publication Date: 2024-11-29EESAVYASA TECHNOLOGIES PVT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032795.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-05
Filing Date
2023-02-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art cannot effectively, economically and environmentally friendly to recover iron values ​​from bauxite residues (red mud), resulting in low recovery rate and high energy consumption in the process. The iron in red mud exists in the form of goiterite, which is strong magnetic for conventional Select no response.

Method used

Induction heating technology is used to selectively heat the iron nanoparticles in the red mud, convert hematite and goite into magnetite, and separate magnetic materials from non-magnetic materials through magnetic separators, and iron recovery is achieved using the principle of magnetic induction.

Benefits of technology

The iron value of 65% to 75% is achieved from the red mud, and a synthetic magnetite black powder is produced for industrial manufacturing applications, improving recycling efficiency and robustness and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053714A_ABST
    Figure CN119053714A_ABST
Patent Text Reader

Abstract

The invention relates to a novel process for recovering iron from bauxite residues. The process comprises directly drying red mud or drying neutralized or washed red mud. Heating in a muffle furnace or an induction furnace at 700 DEG C to 800 DEG C, and treating the bauxite residue with iron nanoparticles having a size of 100 nm to 1000 nm. The surface of the selected substance is coated with the iron particles, so that the magnetism of the selected substance is increased. Iron oxides Fe2O3 and alpha-FeOOH (goethite) existing in the bauxite residues are converted into Fe3O4 (magnetite) after being subjected to induction heating treatment. Therefore, the susceptibility of the particles is improved, and the particles can be separated by a magnetic separator and ultimately separated from a non-magnetic material. In addition, the separated iron-rich material is useful in a variety of applications, such as reduction of arsenic and chemical oxygen demand (COD) in wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an efficient process for recovering iron values ​​from red mud using nanotechnology to produce useful products. Background Art

[0002] Bauxite residue (i.e. red mud) is a solid waste generated in the process of producing alumina from bauxite. Almost 50% of the ore is discarded in the form of red mud, which is the insoluble residue left after the process of digesting bauxite with NaOH. Red mud is a large amount of hazardous waste and is usually stored or dumped with little or no treatment. About 3 billion tons of red mud are dumped or stored worldwide. Red mud is a hazardous waste because it is corrosive and has fine particles and is in powdery form. The dust particles of bauxite residue are very harmful and belong to the category of PM 10 particles that cause silicosis, asthma, lung cancer, and PM 2.5 particles that cause cardiovascular diseases and accumulate in the body. In addition, the metal hydroxides in red mud, together with the residual alkalinity of caustic soda and the leachate, penetrate into the soil, pollute the drinking water / natural water base, and indirectly pollute agriculture. The typical composition of bauxite residue produced during processing on the east coast of India contains 40%-55% Fe2O3, 15%-17% Al2O3, 4%-5% silica, TiO2 and 3%-4% Na2O. Most of the material in red mud is a mixture of Fe2O3 and Al2O3, both of which have a similar crystal structure described as rhombohedral. The similarity of the crystal structure of these two compounds leads to mutual influence, making it difficult to separate the compounds.

[0003] Over the years, several efforts have been made for metallurgical and non-metallurgical applications of bauxite residues, especially for the extraction of iron values. Direct magnetic separation, pyrometallurgical processes and hydrometallurgical processes are the main routes that have been developed to recover iron from red mud. So far, there is no unique solution that is economically or environmentally sustainable. Existing methods are inefficient due to laborious processes, high energy consumption, and the iron in red mud is in the form of goethite, which does not respond to conventional strong magnetic separation, resulting in poor recovery.

[0004] Therefore, in view of the above, there is a need for methods and systems that provide a simple and robust process for recovering iron values ​​from bauxite residues (ie, red mud).

[0005] Purpose of the Invention

[0006] The object of the present invention is to provide a simple and robust process for extracting iron value from bauxite residue. The dried bauxite residue is heated using induction heating. Hematite and goethite in the residue are converted into magnetite, which is separated using a magnetic separator. The non-magnetic material is used to make other useful materials.

[0007] Another object of the present invention is to provide an efficient process for producing iron values ​​by selectively heating bauxite residue with iron nanoparticles followed by magnetic separation. Summary of the invention

[0008] A simplified overview of one or more embodiments is presented below to provide a basic understanding of such embodiments. This content is not an extensive overview of all contemplated embodiments, and is neither intended to identify the key or important elements of all embodiments, nor to describe the scope of any or all embodiments. Its sole purpose is to present some concepts of one or more embodiments in a simplified form as a prelude to a more detailed description presented later.

[0009] An aspect of the present invention is to address at least the above problems and / or disadvantages and to provide at least the advantages described below.

[0010] One aspect of the present invention is a method for processing red mud (RM) to recover iron value. The method neutralizes the red mud with water or acid or acidic waste, followed by a filtration process to remove dissolved salts from the slurry. Further, the method dries the red mud in an oven at a temperature range of 80°C to 100°C for 15 to 18 hours, and further crushes the dried red mud powder into fine particles. And further, the method treats the dried red mud powder with a variety of iron nanoparticles so that the iron oxide (iron oxide) (Fe2O3 and α-FeOOH) in the red mud is converted into magnetite (synthetic Fe3O4), wherein the iron nanoparticles mixed with the red mud are selectively heated by using an induction heating technique to magnetize the iron oxide (ferric oxide) present in the red mud. In addition, the method also separates the magnetic material from the non-magnetic material in the treated red mud by a magnetic separator working on the principle of magnetic induction.

[0011] Another aspect of the present invention is a system for processing red mud (RM) to recover iron values. The system includes: a washing chamber for neutralizing the red mud with water or acid or acidic waste, followed by a filtration process to remove dissolved salts from the slurry; further, a drying chamber for drying the red mud in an oven at a temperature range of 80°C to 100°C for 15 hours to 18 hours; further, a crusher configured to grind the dried red mud to a predetermined particle size; further, a treatment chamber for treating the dried red mud powder with a plurality of iron nanoparticles, wherein the iron oxides (Fe2O3 and α-FeOOH) in the red mud are converted into magnetite (synthetic Fe3O4), wherein the iron nanoparticles mixed with the red mud are selectively heated by using an induction heating technique to magnetize the iron oxides present in the red mud. And, the system may also have one or more separators for separating magnetic materials from non-magnetic materials in the treated red mud by a magnetic separator working on the principle of magnetic induction. All system components may be encapsulated in a housing.

[0012] Other aspects, advantages, and salient features of the invention will become apparent to those skilled in the art from the following detailed description, which, taken in conjunction with the annexed drawings, discloses exemplary embodiments of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Embodiments of the present invention will be discussed with reference to the accompanying drawings, in which:

[0014] Figure 1 A flow chart showing an exemplary method for processing red mud according to an exemplary embodiment of the present invention is shown.

[0015] Figure 2 A schematic configuration of an exemplary system for processing RM according to one embodiment of the present invention is shown.

[0016] Figure 3 Shows Figure 2 An overview of the method defined in the flow chart.

[0017] It should be noted that these drawings are intended to illustrate the general features of the disclosed method and to supplement the written description provided below. Therefore, as will be understood by those skilled in the art, these drawings do not reflect the structural or logical arrangement of the unit operations and equipment that can be used to practice the disclosed method and should not be interpreted as overly limiting or restricting the appended claims. In fact, under the guidance of the present disclosure, it is within the skill of ordinary technicians in the art to design all necessary auxiliary equipment and materials to practice the disclosed method. Similarly, it is within the skill of ordinary technicians in the art to modify and / or adjust the parameters of the disclosed method to compensate for changes in materials, equipment and / or process goals. DETAILED DESCRIPTION

[0018] The following description is provided with reference to the accompanying drawings to assist in a comprehensive understanding of the exemplary embodiments of the present invention as defined by the claims and their equivalents. It includes a number of specific details to assist in understanding, but these are considered exemplary only. Therefore, it will be appreciated by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present invention. In addition, for clarity and brevity, descriptions of well-known functions and structures are omitted.

[0019] The terms and words used in the following description and claims are not limited to the written meanings, but are only used by the inventor to enable a clear and consistent understanding of the present invention. Therefore, it is apparent to those skilled in the art that the following description of exemplary embodiments of the present invention is provided for illustrative purposes only and is not intended to limit the present invention as defined by the appended claims and their equivalents.

[0020] As used herein, the terms "red mud" and "red sludge" refer to the solid waste of the Bayer process for refining bauxite to provide alumina. Red mud is a waste generated by the aluminum manufacturing industry. Red mud generally has the following general composition: Fe2O3 - 30% to 60%, Al2O3 - 10% to 20%, SiO2 - 3% to 50%, Na2O - 2% to 10%, CaO - 2% to 8%, and TiO2 - 0% to 10%. "Red mud residue" or "analogs" mentioned herein refer to other ores or materials having a similar composition to red mud.

[0021] As used herein, the term "about" when used in reference to a process parameter or value means that the value is within at least ±10% of the stated value.

[0022] It should be understood that the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a component surface" includes reference to one or more of such surfaces.

[0023] The term "substantially" means that the characteristic, parameter or value described need not be achieved precisely, but deviations or changes can occur by an amount that does not impair the effect that the characteristic is intended to provide, including, for example, tolerances, measurement errors, measurement precision limitations and other factors known to those skilled in the art.

[0024] Those skilled in the art will appreciate that the principles of the present disclosure can be implemented in any appropriately arranged system. The terms used to describe the various embodiments are exemplary. It should be understood that these are provided only to help understand the specification, and their use and definition in no way limit the scope of the present invention. Unless otherwise expressly stated, the terms first, second, etc. are used to distinguish objects with the same terms and are in no way intended to represent a temporal order. A set is defined as a non-empty set containing at least one element.

[0025] The present invention utilizes a physical process by which the iron oxides (Fe2O3 and α-FeOOH) contained in red mud are converted into synthetic Fe3O4 (magnetite) and further separated for recovery and reuse. The process involves a nanotechnology-based heating device to efficiently and uniformly heat the bauxite residue, which is very fast and energy-efficient. When performed according to the disclosed steps, the method is capable of extracting 65% to 75% of the iron (Fe) in red mud. The product form of iron, synthetic magnetite, is a black powdered material that is widely used as a pigment in industrial manufacturing applications (including high temperature composites, coatings acrylic and oil-based paints, plastics and other polymer resins), and for adding color to various types of metal surfaces.

[0026] The present invention provides a simple and robust process for recovering iron value from bauxite residue. The iron oxides (goethite and hematite) in the bauxite residue are converted into magnetite using nanotechnology. The iron oxides in the red mud are magnetized by selectively heating the iron nanoparticles mixed with the red mud using induction heating technology. It includes the use of iron nanoparticles and induction heating, followed by separation of magnetic materials from non-magnetic materials by a magnetic separator.

[0027] Figure 1 A flow chart of an exemplary method for processing red mud according to an exemplary embodiment of the present invention is shown. In the method of step 110, the red mud is neutralized with water or acid or acid waste, followed by a filtration process to remove dissolved salts from the slurry. Red mud is a by-product of alkaline cooking of bauxite, which is alkaline in nature and remains after the production of pure alumina. It is preferred to use thick red mud collected and deposited in ponds. Alkaline water shows a total dissolved salt of 1000 ppm to 2000 ppm. Wash several times to remove dissolved salts from the slurry, and dry the solid red mud.

[0028] In step 120 , the method dries the bauxite residue (red mud) sample in an oven at a temperature ranging from 80° C. to 100° C. for 15 to 18 hours. Further, in step 130 , the dried powder is crushed into fine particles.

[0029] In step 140, the method treats the dried red mud powder with a plurality of iron nanoparticles so that the iron oxides (Fe2O3 and α-FeOOH) in the red mud are converted into magnetite (synthetic Fe3O4). The iron oxides present in the red mud are magnetized by selectively heating the iron nanoparticles mixed with the red mud using an induction heating technique. In an exemplary embodiment, the dried red mud powder is treated or mixed with a plurality of iron nanoparticles and heated in an induction furnace or a muffle furnace, preferably an induction furnace. The size of the iron nanoparticles can be 100nm to 1000nm, preferably 100nm to 300nm.

[0030] In step 150, the method separates magnetic materials from non-magnetic materials in the treated red mud by a magnetic separator operating on the principle of magnetic induction. In an exemplary embodiment, the mixture is heated to 400° C. to 1000° C. using an induction furnace or a muffle furnace. The preferred temperature is 600° C. to 700° C.

[0031] Conventionally, magnetization is performed by passing through two magnetic separators connected in series, where in the first magnetic separator, a strong magnetic field will magnetize.Hematite or other iron oxides present in the raw red mud sample do not exhibit any magnetic properties.

[0032] In an exemplary embodiment, the iron oxides (Fe2O, Fe2O3, FeOOOH) present in the red mud are magnetized without any washing or neutralization. In another embodiment, the red mud is pre-washed with water to remove soluble salts and subjected to the described process of the invention. The solid is further magnetized using induction heating and a variety of nanocarriers.

[0033] In another embodiment, the red mud is magnetized by heating in an induction furnace. The induction furnace not only serves as a heat source, but also is used to induce an alternating frequency magnetic field suitable for magnetizing the paramagnetic hematite to a magnetic state.

[0034] The red mud containing various forms of iron oxide particles is magnetized using induction heating at a voltage of 380V to 450V and a frequency of 50Hz to 1000Hz, but ideally using an alternating current of about 700kHz to 800kHz and a magnetic separator having a magnetic field power of about 1 Tesla to 1.5 Tesla.

[0035] Preferably, the induction heating is performed using a crucible selected from iron, stainless steel, graphite and ceramics because, immediately following the change in the structure of the red mud, the initially paramagnetic hematite particles are pre-magnetized by the induced magnetic field of the crucible, which is an important step in changing the hematite particles to a magnetic state.

[0036] After the red mud is treated using the innovative process of the present invention, it is treated by a magnetic separator, which is preferably a device for separating magnetic materials from non-magnetic materials operating on the principle of magnetic induction, or is designed to be the same as a device with a "magnetization" function. The magnetic separator is a machine with a sufficiently high productivity to be able to separate magnetic materials from non-magnetic materials in the red mud powder.

[0037] In another embodiment, the treated red mud containing magnetite formed by goethite and hematite shows a higher percentage of total iron content. In this process, goethite (α-FeOOH) and magnetic hematite (Fe2O3, γ-Fe2O3) in one of the red mud samples are converted to Fe3O4 in the form of magnetite ferrous ferric oxide. This does not adversely affect the excellence and efficiency of the magnetic separation process.

[0038] For the above process or method, induction heating is preferably used. On the one hand, such a heater and the temperature achieved therewith are well controllable. On the other hand, the induction furnace also induces an alternating frequency magnetic field suitable for magnetizing hematite to magnetite.

[0039] Chemical conversion or thermal processes as previously described in the reported methods (preparation of magnetite from hematite and goethite) are not perfect. These methods require stronger magnetic fields to separate the magnetic material from the non-magnetic material. Although there are reports of magnetizing crude red mud from hematite to magnetite, this is unreliable and non-renewable, and most importantly, it is not commercially viable.

[0040] For the implementation of the process, crucibles such as graphite, ceramic, stainless steel, iron are suitable, which are heated by industrial electricity at 380 V, 500 Hz to 100 Hz, while the heating power is controlled by setting the desired temperature.

[0041] In one embodiment of the invention, red mud is treated with water to remove soluble salts.

[0042] The slurry was dried in a hot air oven at 90°C to 100°C for 18 hours to 24 hours. The moisture content showed a pH of 9.0 to 11.0, total dissolved salts of 1000 ppm to 3000 ppm, and a conductivity of 2 mSv to 4 mSv.

[0043] In one embodiment of the process of the present invention, dried red mud is mixed with iron nanoparticles having a size range of 100 nm to 1000 nm and heated in an induction furnace. The frequency used is in the range of 200 Hz to 800 Hz. The voltage used is in the range of 250 V to 450 V. The current required for the process is in the range of 50 A to 100 A. The furnace temperature is 300° C. to 1000° C., preferably 700° C. to 8000° C. is used.

[0044] In another embodiment of the process according to the invention, the remaining slurry is neutralized by acid treatment in dilution water in a weight ratio of 1:2, preferably a weight ratio of 1.3 to 1.5, and then stirred at 40°C to 90°C, preferably 60°C-80°C for 0.5 to 3 hours, preferably 1 to 2 hours. To neutralize the slurry, a portion of a strong acid, in particular 96% industrial strength sulfuric acid, is added under stirring, during which the mixture reaches a neutral state of about pH = 7. The filtered solution containing the soluble salts of the rare earth metal sulfate is separated, for example, by decantation, suction or centrifugation, and the solution is evaporated in whole or in part at a temperature of up to 100°C.

[0045] The solid is dried and used in the process by mixing iron nanoparticles and heating in an induction furnace or muffle furnace. Goethite and hematite are converted into magnetite. The total iron content is significantly increased compared to the original red mud.

[0046] The magnetite iron oxide produced by the process of the present invention is used in a variety of applications. For example, it is used in water treatment to remove arsenic from water, remove COD from pharmaceutical wastewater, textile wastewater, etc. Other examples of application areas include as a catalyst, pigment, and metallurgical recovery.

[0047] Finally, it should be noted that the device according to the invention for use in the chemical industry is easy to design, so the functional design, material selection, and dimensioning of the unit belong to routine work for ordinary technicians in the field, and therefore will not be discussed in detail in the description of this specification.

[0048] analyze

[0049] X-ray crystallography

[0050] The crystal phase of the sample was determined by X-ray diffraction (XRD). XRD measurements were performed using a diffractometer XRD7000 (Shimadzu) with an observation system via BraggBrettano in filtered emission CuKα (λ = 0.154184 nm) and CoKα (λ = 0.179026 nm). XRD phase diagnosis was performed using a diffraction data card by detecting the d spacing (using Cu-K radiation, a scanning speed of 8 ° / min, and a scanning range of 50° to 85°).

[0051] Dynamic Light Scattering (DLS) and Zeta Potential

[0052] Particle size and zeta potential were measured using a Horiba SZ100 (HORIBA India Private Limited). DLS uses a high energy laser light source and a sensitive detector that has scattering information in particle size measurements at 90° and 173°. HORIBA includes the most sensitive PMT detector available.

[0053] Chemical Analysis of Bauxite Residue Samples

[0054] Sample 1: Total iron content 29.5%, XRD-hematite (49.0%), goethite (23.0%), magnetite (5.0%).

[0055] Sample 2: Total iron content 12%, XRD-hematite (46.8%), maghemite (21.6%), goethite (28.6%), magnetite (3.1).

[0056] Example

[0057] Example 1

[0058] The raw red mud was dried in a vacuum oven overnight. The dried powder (100 g) was heated in a crucible using induction heating. The temperature was maintained at 700°C to 800°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 33.1%.

[0059] Example 2

[0060] The raw red mud was dried in a vacuum oven overnight. The dried powder (99 g) was mixed with iron powder (1 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 800 Hz, and the temperature was maintained at 700 ° C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 34.4%.

[0061] Example 3

[0062] The dried powder (98 g) was mixed with iron powder (2 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 800 Hz, and the temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 35.1%.

[0063] Example 4

[0064] The dried powder (97 g) was mixed with iron powder (3 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 800 Hz, and the temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 36.4%.

[0065] Example 5

[0066] The dried powder (95 g) was mixed with iron powder (5 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 800 Hz, and the temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 43.9%.

[0067] Example 6

[0068] The dried powder (95 g) was mixed with iron powder (5 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 900 Hz to 100 Hz, and the temperature was maintained at 900°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 46.9%.

[0069] Example 7

[0070] The raw red mud was dried overnight in a vacuum oven. The dried powder (100 g) was heated in a crucible using a muffle furnace. The temperature was maintained at 700°C for 30 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 32.1%.

[0071] Example 8

[0072] The raw red mud was dried overnight in a vacuum oven. The dried powder (99 g) was mixed with iron powder (1 g, grade A, see below) and heated in a crucible using a muffle furnace. The temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 32.6%.

[0073] Example 9

[0074] The raw red mud was dried overnight in a vacuum oven. The dried powder (97 g) was mixed with iron powder (3 g, grade A, see below) and heated in a crucible using a muffle furnace. The temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 33.2%.

[0075] Example 10

[0076] The dried powder (95 g) was mixed with iron powder (5 g, grade A, see below) and heated in a crucible using induction heating. The voltage was 440 V, the frequency was 800 Hz, and the temperature was maintained at 700°C for 45 minutes. After treatment, the reaction mixture was cooled to room temperature and analyzed by chemical and physical methods. Total iron content: 35.6%.

[0077] Embodiment 11

[0078] The treated red mud (100 g) in Example 5 was washed with water (2 x 100 mL), filtered and dried. The weight obtained was (95 g). The dried powder was used to reduce arsenic and remove COD from water. Red mud (1 g) was added to 100 mL of arsenic solution with a concentration of 500 ppb and stirred for 1 hour. After filtration, the solution was tested for arsenic, and the arsenic content was 50 ppb. In the second experiment, 5 g of red mud powder was taken, 100 mL of pharmaceutical wastewater (COD 24500 ppm) was added, and stirred for 2 h. The COD after treatment was 11800 ppm.

[0079] Figure 2 A schematic configuration of an exemplary system for processing red mud (RM) according to one embodiment of the present invention is shown. The system mainly includes a washing chamber, a drying chamber, a crusher, a treatment chamber, and one or more separators. The system is generally enclosed in a housing that at least partially encloses the washing chamber, the drying chamber, the crusher, the treatment chamber, and at least one of the one or more separators.

[0080] In the configuration of the exemplary embodiment, the washing chamber is used to neutralize the red mud with water or acid or acidic waste, followed by a filtration process to remove dissolved salts from the slurry. The drying chamber is used to dry the red mud in an oven at a temperature range of 80°C to 100°C for 15 to 18 hours. The crusher is configured to grind the dried red mud to a predetermined particle size. The treatment chamber is used to treat the dried red mud powder with a variety of iron nanoparticles to convert the iron oxides (Fe2O3 and α-FeOOH) in the red mud into magnetite (synthetic Fe3O4), wherein the iron nanoparticles mixed with the red mud are selectively heated by using an induction heating technique to magnetize the iron oxides present in the red mud. The magnetic material in the treated red mud is separated from the non-magnetic material by a magnetic separator working on the principle of magnetic induction.

[0081] Figure 3 Shows Figure 1 An overview of the method defined in the flow chart.

[0082] Those skilled in the art will appreciate that the present invention is not limited in its application to the specific application described. The present invention is also not limited to the preferred embodiments with respect to the specific elements and / or features described or depicted herein. It should be understood that the present invention is not limited to the disclosed one or more embodiments, but is capable of many rearrangements, modifications and substitutions without departing from the scope of the present invention as set forth and defined by the appended claims.

[0083] Unless the context requires otherwise, throughout the specification and the appended claims, the words "comprise" and "comprising" and variations such as "containing" and "having", will be understood to imply the inclusion of stated integers or groups of integers but not the exclusion of any other integers or groups of integers.

[0084] The reference to any prior art in this specification is not, and should not be taken as, an admission that such prior art forms part of the common general knowledge.

Claims

1. A method for processing red mud (RM) to recover iron values, comprising: neutralizing the red mud with water or acid or acidic waste followed by a filtration process to remove dissolved salts from the slurry; Drying the red mud in an oven at a temperature ranging from 80° C. to 100° C. for 15 to 18 hours, and further crushing the dried red mud powder into fine particles; treating the dried red mud powder with a plurality of iron nanoparticles such that the iron oxides (Fe2O3 and α-FeOOH) in the red mud are converted into magnetite (synthetic Fe3O4), wherein the iron nanoparticles mixed with the red mud are selectively heated by using an induction heating technique to magnetize the iron oxides present in the red mud; as well as The magnetic materials in the treated red mud are separated from the non-magnetic materials by a magnetic separator working on the principle of magnetic induction.

2. The method according to claim 1, wherein: The size of the iron nanoparticles is 100 nm to 1000 nm, and preferably 100 nm to 300 nm.

3. The method according to claim 1, wherein: The selective heating is performed using an induction furnace in a temperature range of 400°C to 1000°C, and preferably at a temperature of 600°C to 700°C.

4. The method according to claim 1, wherein: The magnetization is carried out by passing through two magnetic separators connected in series, wherein a strong magnetic field for magnetization is provided in the first magnetic separator.

5. The method according to claim 1, wherein: The induction furnace also induces an alternating frequency magnetic field suitable for magnetizing the paramagnetic hematite to a magnetic state.

6. The method according to claim 1, wherein: The induction heating has a voltage range of 380V to 450V, a frequency range of 50Hz to 1000Hz, with a preferred range of 800kHz AC, and the magnetic separator has a magnetic field power of about 1 Tesla to 1.5 Tesla.

7. The method according to claim 1, wherein: The structure of the red mud is changed by induction heating, and the initially paramagnetic hematite particles are pre-magnetized by the induced magnetic field of the induction heating so that the hematite particles change to a magnetic state.

8. The method according to claim 1 is capable of extracting 65% to 75% of the iron (Fe) in the red mud, wherein the product form of the iron, synthetic magnetite, is a black powdered material, and the synthetic magnetite is widely used as a pigment in industrial manufacturing applications, including high temperature composites, coatings acrylic and oil-based paints, plastics and other polymer resins; and the synthetic magnetite is used to add color to various types of metal surfaces.

9. The method according to claim 1, wherein: The treated red mud containing magnetite formed from goethite and hematite showed a higher percentage of total iron content.

10. The method according to claim 1, wherein: The treated red mud is washed with water at room temperature to 100°C to remove soluble salts.

11. A system for processing red mud (RM) to recover iron values, comprising: a washing chamber for neutralizing the red mud with water or acid or acidic waste followed by a filtration process to remove dissolved salts from the slurry; A drying chamber for drying the red mud in an oven at a temperature ranging from 80° C. to 100° C. for 15 to 18 hours; a crusher configured to grind the dried red mud to a predetermined particle size; a treatment chamber for treating dried red mud powder with a plurality of iron nanoparticles such that iron oxides (Fe2O3 and α-FeOOH) in the red mud are converted into magnetite (synthetic Fe3O4), wherein the iron nanoparticles mixed with the red mud are selectively heated by using an induction heating technique to magnetize the iron oxides present in the red mud; as well as One or more separators for separating magnetic material from non-magnetic material in the treated red mud by means of a magnetic separator operating on the principle of magnetic induction.

12. The system according to claim 12, further comprising: A housing at least partially encloses the washing chamber, the drying chamber, the crusher, the processing chamber, and at least one of the one or more separators.