Adhesive tape for dicing
By using the cutting adhesive tape with low melting point and surface roughness control, the problem of reduced transmittance and insufficient expansion under heating of the cutting adhesive tape is solved, and high-precision invisible cutting and efficient cutting are achieved.
Patent Information
- Application Number
- CN202480001615.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-29
AI Technical Summary
The existing cutting adhesive tape has a reduced transmittance after vacuum adsorption under heating, resulting in a deterioration of invisible cutting accuracy and insufficient expansion of high heat-resistant materials, which affects cutting efficiency.
The base material film with a melting point of 150°C or less is used, and the surface roughness Ra of the base material film is controlled to be less than 0.10μm and the needle temperature is more than 80°C to ensure that it is maintained after vacuum adsorption under heating. High transmittance and excellent expansion when extended cut.
The high transmittance to the laser after vacuum adsorption under heating is achieved, ensuring high accuracy of invisible cutting, and maintaining excellent expansion when expanding cutting, improving the cutting efficiency of semiconductor chips.
Smart Images

Figure CN119054050A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive tape for dicing. Background Art
[0002] Before a semiconductor wafer is processed into a semiconductor chip and installed in a semiconductor device such as an integrated circuit (IC), the following steps are included, for example: a step of attaching a semiconductor wafer surface protection tape or a back grinding substrate to the patterned surface of the semiconductor wafer; a step of grinding the back of the semiconductor wafer to reduce the thickness; a step of installing the thinned semiconductor wafer on a dicing adhesive tape; a step of peeling off the above-mentioned semiconductor wafer surface protection tape or back grinding substrate from the semiconductor wafer; a step of dividing the semiconductor wafer by dicing; a picking up step of picking up the divided semiconductor chips; a bonding step of joining the picked up semiconductor chip to a lead frame; a molding step of encapsulating the semiconductor chip after the bonding step with resin; etc.
[0003] The dicing adhesive tape functions as a support for the semiconductor chip not only in the dicing step but also in the pickup step.
[0004] A method of performing the above-mentioned dicing process by laser irradiation is known. Specifically, the following method is known: by irradiating the laser from the side of the dicing tape, a modified region serving as a starting point for division is formed inside the semiconductor wafer, and then the dicing tape is expanded to cut the modified region and separate into semiconductor chips. This dicing method is called stealth dicing. In stealth dicing, in order to perform high-precision laser irradiation on the wafer and to enable appearance inspection, etc., the dicing tape is required to have high transparency.
[0005] Patent document 1 proposes an adhesive sheet for stealth dicing, which is an adhesive sheet for stealth dicing having a substrate and an adhesive layer laminated on one side of the substrate, wherein, when the substrate is stretched with a load of 0.2 g while being heated from 25°C to 120°C at a heating rate of 20°C / min using a thermomechanical analysis device, the change in the substrate obtained by subtracting the initial length of the substrate from the length of the substrate at 60°C is set as ΔL 60℃ The change in the substrate obtained by subtracting the initial length of the substrate from the length of the substrate at 90° C. is defined as ΔL. 90℃ When , the formula (1) is satisfied: ΔL 90℃ -ΔL 60℃ <0 μm. According to Patent Document 1, it is believed that the adhesive sheet for stealth dicing has excellent heat shrinkage.
[0006] Patent document 2 proposes a cutting sheet, which is a cutting sheet having a substrate and an adhesive layer laminated on the first surface side of the substrate, wherein the arithmetic mean roughness (Ra) of the second surface of the substrate is greater than 0.01 μm and less than 0.5 μm, and the maximum height (Rz) of the profile of the second surface of the substrate is less than 3 μm. The cutting sheet has light transmittance suitable for high-magnification photography of a workpiece.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2018 / 083986
[0010] Patent Document 2: International Publication No. 2018 / 084021 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, as a method for mounting a semiconductor chip on a wiring substrate, a flip chip connection is known. In this flip chip connection, a resin is filled between the semiconductor chip and the wiring substrate. Considering the work efficiency, the filled resin is made into an adhesive film such as NCF (Non Conductive Film) and attached to the wafer before dicing, and singulated at the same time as the wafer.
[0013] In the method using such an adhesive film, after laminating the dicing tape on the wafer, the adhesive film is laminated on the surface of the wafer to which the dicing tape is not laminated. More specifically, the lamination is performed as follows. The laminate of the dicing tape and the wafer is arranged on a chuck table (CT) heated to about 80°C in such a manner that the dicing tape side contacts the chuck table, and fixed by vacuum adsorption. In this fixed state, the adhesive film is laminated on the side of the wafer opposite to the dicing tape side. The inventors of the present invention conducted a study and found that after the above-mentioned fixation, the transmittance of the dicing tape is easily reduced. If a dicing tape with reduced transmittance is used, meandering of the modified area will occur in the subsequent stealth dicing process, and the processing accuracy will easily deteriorate.
[0014] It is believed that the reduction in the above transmittance is due to the vacuum adsorption at high temperature causing the surface of the chuck table to be transferred to the cutting adhesive tape, making the back of the cutting adhesive tape rough. This problem can be improved by improving the heat resistance (melting point, etc.) of the base film constituting the cutting adhesive tape. However, high heat-resistant materials are usually highly rigid, and the cutting adhesive tape using high heat-resistant materials has the problem of reduced expansion (elongation) of the cutting adhesive tape when it is extended and cut.
[0015] The present invention has been made in view of the problems existing in the above-mentioned prior art, and its object is to provide a dicing adhesive tape which shows sufficiently high transmittance to laser light even after being vacuum-adsorbed on a chuck table under heating, and has excellent expandability during expansion cutting.
[0016] Means for solving problems
[0017] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by setting the penetration temperature to a specific temperature or higher and controlling the surface roughness to a specific value or lower even when a resin with a low melting point is used for the base film of the dicing pressure-sensitive adhesive tape.
[0018] That is, the above-mentioned problems of the present invention are solved by the following means. [1]
[0020] A cutting adhesive tape having an adhesive layer on a substrate film, wherein the melting point of the substrate film is below 150°C, the surface roughness Ra of the surface A of the substrate film opposite to the adhesive layer is below 0.10 μm, and the needle penetration temperature of the surface A is above 80°C. [2]
[0022] The dicing pressure-sensitive adhesive tape according to [1], wherein the base film has no yield point before the elongation reaches 50% in a stress-elongation curve at -15°C. [3]
[0024] The cutting adhesive tape as described in [1] or [2], wherein the absolute value of the difference between the stress (MD stress, S1) (MPa) of the substrate film at an elongation of 30% when stretched in the MD direction in a tensile test at -15°C and the stress (TD stress, S2) at an elongation of 30% when stretched in the TD direction is 4 MPa or less. [4]
[0026] The cutting adhesive tape as described in any one of [1] to [3], wherein the substrate film is composed of at least two layers, and the relationship between the needle penetration temperature (T1) of the surface on which the adhesive layer is formed and the needle penetration temperature (T2) of the surface on which the adhesive layer is not formed satisfies [(T2)-(T1)]>0°C. [5]
[0028] The dicing pressure-sensitive adhesive tape according to any one of [1] to [4], wherein the base film comprises at least one of an ethylene-alkyl (meth)acrylate copolymer resin and an ionomer resin. [6]
[0030] The pressure-sensitive adhesive tape for dicing as described in any one of [1] to [5], which is a stealth pressure-sensitive adhesive tape for dicing.
[0031] In the present invention, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0032] In the present invention, (meth)acrylic acid refers to one or both of acrylic acid and methacrylic acid. The same applies to (meth)acrylate.
[0033] In the present invention, the MD direction is the flow direction of the film during film formation, and the TD direction is the direction perpendicular to the MD direction.
[0034] Effects of the Invention
[0035] The dicing pressure-sensitive adhesive tape of the present invention exhibits sufficiently high transmittance to laser light even after being vacuum-adsorbed on a chuck table under heating, and is also excellent in expandability during expansion dicing. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a cross-sectional view showing one embodiment of the dicing pressure-sensitive adhesive tape of the present invention.
[0037] Figure 2 This is a schematic longitudinal cross-sectional view of an adhesive film laminating step in a preferred embodiment of a method for manufacturing a semiconductor device using the dicing adhesive tape of the present invention.
[0038] Figure 3 This is a schematic longitudinal cross-sectional view showing a state after peeling off the release film according to a preferred embodiment of a method for manufacturing a semiconductor device using the dicing pressure-sensitive adhesive tape of the present invention.
[0039] Figure 4 This is a schematic longitudinal cross-sectional view showing a preferred embodiment of a method for manufacturing a semiconductor device using the dicing adhesive tape of the present invention, in a state after being unloaded from a chuck table.
[0040] Figure 5 This is a schematic longitudinal cross-sectional view of a modified region forming step in a preferred embodiment of a method for manufacturing a semiconductor device using the dicing adhesive tape of the present invention.
[0041] Figure 6 This is a schematic longitudinal cross-sectional view showing a state after heat shrinkage according to a preferred embodiment of a method for manufacturing a semiconductor device using the dicing adhesive tape of the present invention.
[0042] Figure 7 It is an explanatory diagram showing the measurement points of the incision width in the evaluation of the examples and comparative examples. DETAILED DESCRIPTION
[0043] The adhesive tape for dicing of the present invention (hereinafter also referred to as "the adhesive tape of the present invention") comprises a substrate film and an adhesive layer. The adhesive tape of the present invention is used as a so-called dicing film. The adhesive tape of the present invention is suitable as an invisible dicing adhesive tape having expandability and heat shrinkability.
[0044] In the adhesive tape of the present invention, the melting point of the substrate film measured by differential scanning calorimetry (DSC) is 150° C. or less. In addition, the surface of the substrate film opposite to the adhesive layer has a surface roughness Ra of 0.10 μm or less. Furthermore, the needle penetration temperature of the surface of the substrate film opposite to the adhesive layer is 80° C. or more.
[0045] The adhesive tape of the present invention is not easy to transfer the unevenness of the chuck table surface even when the adhesive film is adhered to the semiconductor wafer (hereinafter also referred to as "wafer") by heating (for example, heating at a temperature of 80°C or more for several minutes) before dicing, so that the laser transmittance can be fully maintained even after vacuum adsorption on the chuck table under heating, and as a result, the formation of the modified area based on laser irradiation from the adhesive tape side can be performed with high precision. In addition, the expansion property in the expansion process after dicing is also excellent, which can further improve the efficiency of cutting the wafer into wafer chips (semiconductor chips).
[0046] Furthermore, according to the preferred embodiment of the present invention, during heat shrinkage, more uniform heat shrinkage can be performed, and the slit widths in the MD and TD directions can be more easily set to appropriate ranges.
[0047] Figure 1 1 is a cross-sectional view of an embodiment of the adhesive tape 10 of the present invention, showing an embodiment of the present invention. The adhesive tape 10 of the present invention has a base film 11 and an adhesive layer 12. When the adhesive tape 10 of the present invention is used, the back of the wafer is bonded to the adhesive layer 12. It should be noted that the adhesive layer 12 can be pre-cut (pre-cut) into a predetermined shape according to the use process and device. The adhesive tape 10 of the present invention can be in a form cut for each wafer, or in a form in which a long strip of a plurality of wafers cut for each wafer is wound into a roll.
[0048] In the present invention, the adhesive layer refers to a coating layer of the adhesive composition, and the polymer contained in the adhesive is in a state of exerting adhesive force or cohesive force. In addition, when the adhesive layer is energy-ray-curable, the adhesive layer is in a state before being cured by energy-ray irradiation.
[0049] Hereinafter, the configuration of each layer will be described.
[0050] <Base Film>
[0051] The base film 11 may be a single layer or a laminate composed of a plurality of layers. In the case of a laminate, it is preferred that the materials used to form the respective layers are different.
[0052] The melting point of the base film 11 is 150° C. or lower.
[0053] The melting point is preferably 140°C or less, preferably 130°C or less, more preferably 120°C or less, more preferably 110°C or less, further preferably 100°C or less, and particularly preferably 90°C or less. The lower limit is not particularly limited, but is actually 50°C or more, preferably 60°C or more, and further preferably 70°C or more. Therefore, if the melting point of the substrate film 11 is expressed as a preferred range, it is preferably 50 to 150°C, more preferably 50 to 140°C, further preferably 50 to 130°C, further preferably 60 to 120°C, further preferably 60 to 110°C, further preferably 70 to 100°C, and further preferably 70 to 90°C.
[0054] The melting point of the base film 11 can be measured by differential scanning calorimetry (DSC) according to the method described in Examples.
[0055] The melting point of the base film 11 can be set to the above range by controlling the material and layer structure of the base film 11 , blending with other materials, and the like.
[0056] The surface roughness (arithmetic mean roughness) Ra of the surface of the substrate film 11 opposite to the surface on which the adhesive layer 12 is formed (hereinafter sometimes referred to as the "back side") is 0.10 μm or less, preferably 0.08 μm or less, more preferably 0.06 μm or less, and further preferably 0.04 μm or less. The lower limit of the surface roughness Ra of the back side is not particularly limited, and is actually 0.01 μm or more. Therefore, if the Ra of the back side of the substrate film 11 is expressed as a preferred range, it is preferably 0.01 to 0.10 μm, more preferably 0.01 to 0.08 μm, further preferably 0.01 to 0.06 μm, and further preferably 0.01 to 0.04 μm. In the case where the substrate film 11 is composed of multiple layers, the surface roughness Ra of the outermost layer on the back side of the substrate film 11 can be within the above range.
[0057] The surface roughness Ra of the back side of the substrate film 11 can be controlled by the method for preparing the substrate film 11. For example, in the case of the T-die method and the calendaring method, it can be controlled by adjusting the surface roughness of the cooling roller during film extrusion, and in the case of the solution casting method, it can be controlled by adjusting the surface roughness of the roller or the belt.
[0058] The surface roughness Ra of the surface of the base film 11 on which the pressure-sensitive adhesive layer 12 is to be formed is not particularly limited.
[0059] The surface roughness Ra of the base film 11 can be measured according to JIS B0601:2001 by the method described in Examples.
[0060] The needle penetration temperature of the back surface of the substrate film 11 is 80° C. or higher, preferably 83° C. or higher, more preferably 85° C. or higher, more preferably 88° C. or higher, further preferably 90° C. or higher, and particularly preferably 92° C. or higher. The upper limit of the needle penetration temperature of the back surface of the substrate film 11 is preferably 100° C. or lower, more preferably 98° C. or lower, and further preferably 95° C. or lower. Therefore, if the needle penetration temperature of the back surface of the substrate film 11 is expressed as a preferred range, it is preferably 80 to 100° C., more preferably 83 to 98° C., further preferably 85 to 98° C., further preferably 88 to 98° C., further preferably 90 to 95° C., and particularly preferably 92 to 95° C.
[0061] The penetration temperature can be measured by thermomechanical analysis (TMA: Thermomechanical Analysis) in accordance with JIS K7196:2012 by the method described in Examples.
[0062] The needle penetration temperature can be controlled by selecting the material constituting the base film, making the base film composed of multiple layers of different materials, controlling the thickness of the resin layer constituting the laminate, etc. For example, if a material with a high softening starting temperature is used as the material constituting the base film, there is a tendency for the needle penetration temperature to become higher. In addition, when a material with a high softening starting temperature is laminated on the back side of the base film and its thickness is increased, there is a tendency for the needle penetration temperature to become higher. Even when a material with a high softening starting temperature is laminated on the back side of the base film, when the thickness of the layer is thin and the softening starting temperature of the resin of other layers is low, there is a tendency for the needle penetration temperature to become lower.
[0063] If the needle penetration temperature of the back side of the substrate film 11 is above 80°C, even if a material with a low melting point and not too high rigidity is used as the constituent material of the substrate film, it is possible to effectively prevent the unevenness of the chuck table surface from being transferred to the substrate film due to vacuum adsorption at high temperature.
[0064] When the base film 11 is a laminate composed of at least two layers, the relationship between the needle penetration temperature (T1) of the surface on which the adhesive layer 12 is formed and the needle penetration temperature (T2) of the surface (back surface) on which the adhesive layer 12 is not formed is preferably [(T2)-(T1)]>0°C (i.e., T2>T1). Such a base film has excellent heat shrinkage during heat shrinkage. The relationship between T1 and T2 is more preferably [(T2)-(T1)]>20°C, further preferably [(T2)-(T1)]>30°C, further preferably [(T2)-(T1)]>40°C, and particularly preferably [(T2)-(T1)]>50°C. The relationship between T1 and T2 can also be [(T2)-(T1)]>80°C. The upper limit of [(T2)-(T1)] is not particularly limited, and is actually 100°C. Therefore, the relationship between T1 and T2 is preferably 100°C>[(T2)-(T1)]>0°C, more preferably 100°C>[(T2)-(T1)]>20°C, further preferably 100°C>[(T2)-(T1)]>30°C, further preferably 100°C>[(T2)-(T1)]>40°C, further preferably 100°C>[(T2)-(T1)]>50°C.
[0065] The substrate film 11 preferably has no yield point between 0% and 50% elongation in the stress-elongation curve at -15°C. Such a substrate film can be expanded more uniformly (especially cold expanded), and the adhesive tape is not easily broken, and a sufficient incision width can be maintained after heat shrinkage.
[0066] The yield point can be determined by the method described in the examples. In the present invention, the stress-elongation curve is a curve obtained by elongation in the TD direction.
[0067] The substrate film 11 preferably has an absolute value of the difference between the stress (MD stress, S1) (MPa) at 30% elongation when stretched in the MD direction and the stress (TD stress, S2) (MPa) at 30% elongation when stretched in the TD direction in a tensile test at -15°C of 4MPa or less (satisfying 4MPa≥|(S1)-(S2)|). If S1 and S2 satisfy the above relationship, the difference in the incision width in the MD direction and the TD direction after heat shrinkage can be further reduced, which is preferred from this perspective. The absolute value of the difference between S1 and S2 is more preferably 3MPa or less.
[0068] The constituent material of the base film 11 is not particularly limited as long as the above-mentioned melting point, surface roughness Ra, and needle penetration temperature can be achieved.
[0069] It is preferable that the base film 11 has uniform and isotropic expandability because the wafer can be cut uniformly in all directions in the expansion step.
[0070] From these viewpoints, the constituent material of the base film 11 is preferably selected from polyolefin resins and polyvinyl chloride resins.
[0071] Examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymers, poly-1-butene, poly-4-methyl-1-pentene, ethylene-vinyl acetate copolymers, ethylene-(meth)acrylate alkyl ester copolymers (ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-methyl methacrylate copolymers, etc.), ethylene-acrylic acid copolymers, ionomers and other α-olefin homopolymers or copolymers thereof, or mixtures thereof.
[0072] Particularly preferred is a synthetic resin, i.e., an ionomer resin, in which a polymer is made into an aggregate by utilizing the cohesive force generated by metal ions. For example, an ionomer resin obtained by crosslinking an ethylene-(meth)acrylic acid binary copolymer or an ethylene-(meth)acrylic acid-(meth)acrylic acid alkyl ester ternary copolymer with metal ions can be exemplified. They are suitable for the expansion process in terms of uniform expansibility. The metal ions contained in the above-mentioned ionomer resin are not particularly limited, and zinc ions, sodium ions, etc. can be cited. Zinc ions are preferred from the aspects of low solubility and low contamination.
[0073] Generally, ionomer resin has a greater restoring force to stretching than resins without metal ions, and has a greater shrinkage stress when heat is applied in a stretched state after the expansion process. Therefore, ionomer resin is preferred in that a heat shrinking process can be performed, which is to remove the slack generated in the tape by heat shrinking after the expansion process, so that the tape is tightened and the interval between each wafer chip is stably maintained.
[0074] In addition to the above ionomer resins, thermoplastic crosslinked resins obtained by crosslinking a resin selected from low-density polyethylene having a specific gravity of 0.910 or more and less than 0.930, ultra-low-density polyethylene having a specific gravity of less than 0.910, and ethylene-vinyl acetate copolymers are also preferred.
[0075] As a method of cross-linking, there can be cited a method of irradiating the above-mentioned resin with energy rays such as electron beams. Such a thermoplastic cross-linked resin has a certain uniform expansibility because the cross-linked part and the non-cross-linked part coexist in the resin. In addition, such a thermoplastic cross-linked resin contains almost no chlorine atoms in the molecular chain structure, so even if the unnecessary tape is incinerated after use, chlorinated aromatic hydrocarbons such as dioxins and their analogs will not be generated, and the environmental burden is also small. By appropriately adjusting the amount of energy rays irradiated on the above-mentioned polyethylene and ethylene-vinyl acetate copolymer, a resin with sufficient uniform expansibility can be obtained.
[0076] It should be noted that in Figure 1In the example shown, the base film 11 is a single layer, but it is not limited thereto and may be a plurality of layers. The plurality of layers may be a plurality of layers formed by laminating two or more layers composed of different resins, or may be a plurality of layers formed by laminating layers composed of one resin. If the two or more resins are cross-linked resins or non-cross-linked resins, it is preferred from the viewpoint that the characteristics of each are further enhanced and expressed. In the case of laminating a cross-linked resin and a non-cross-linked resin in combination, it is preferred from the viewpoint that the disadvantages of each are compensated.
[0077] As a method for producing the multi-layer base film 11, a common extrusion method, a lamination method, etc. can be used. When the lamination method is used, an adhesive can be interposed between the layers. As the adhesive, a common adhesive can be used.
[0078] The substrate film 11 preferably contains at least one of an ethylene-alkyl (meth)acrylate copolymer resin and an ionomer resin. The substrate film 11 is also preferably a laminate of a layer containing an ethylene-alkyl (meth)acrylate copolymer resin and a layer containing an ionomer resin.
[0079] The thickness of the base film 11 is not particularly limited, but is preferably 50 to 200 μm, more preferably 70 to 160 μm, further preferably 100 to 150 μm, further preferably 100 to 140 μm, further preferably 100 to 120 μm.
[0080] <Adhesive Layer>
[0081] The adhesive layer 12 constituting the adhesive tape 10 of the present invention is not particularly limited as long as it has a property of retaining the adhesive layer to a degree that does not cause peeling from the wafer during the dicing process, a property of transmitting the stress generated by expansion to the modified area of the wafer, and a property of being able to be peeled from the wafer chip during pickup.
[0082] The adhesive constituting the adhesive layer 12 is not particularly limited as long as it exhibits the above-mentioned properties, and is preferably an energy-ray-curable adhesive. If it is an energy-ray-curable adhesive, it is easy to pick up by curing it before the pickup process. Here, energy rays refer to light such as ultraviolet rays, or ionizing radiation such as electron beams.
[0083] As the adhesive constituting the adhesive layer 12, a common adhesive used as an adhesive for a dicing adhesive tape can be used without particular limitation. As for the composition, properties, and manufacturing method of the adhesive, for example, reference can be made to paragraphs
[0039] to
[0076] of Japanese Patent No. 6928852, paragraphs
[0033] to
[0052] of Japanese Patent No. 6989561, and paragraphs
[0031] to
[0057] of Japanese Patent Publication No. 2023-13022.
[0084] The adhesive constituting the adhesive layer 12 is preferably an acrylic adhesive containing a (meth) acrylic resin as a base polymer, and more preferably an acrylic adhesive containing an alkyl (meth) acrylate as a constituent component. The alkyl (meth) acrylate preferably further has a radiation-curable group introduced into the side chain, and more preferably has a (meth) acrylate having an isocyanate group added thereto. The adhesive may further contain a radiation-curable oligomer, such as a urethane (meth) acrylate oligomer, and the like.
[0085] The thickness of the adhesive layer 12 is not particularly limited. If the thickness is 2 μm or more, the adhesive strength is excellent, more preferably 5 μm or more, and more preferably 10 μm or more. If the thickness is 35 μm or less, the pickup property is excellent, and more preferably 30 μm or less. Therefore, the thickness of the adhesive layer 12 is preferably 2 to 35 μm, more preferably 5 to 35 μm, more preferably 5 to 30 μm, and more preferably 10 to 30 μm.
[0086] <Purpose>
[0087] The adhesive tape 10 of the present invention is suitable for use in a method for manufacturing a semiconductor device, which includes at least: an adhesive film laminating step, which includes fixing the adhesive tape 10 on a heated chuck table by vacuum adsorption; a modified region forming step, which forms a modified region in a wafer by irradiating a laser from the adhesive tape side; and an expansion step, which cuts the wafer by expansion. Therefore, other steps, the order of the steps, etc. are not particularly limited. For example, it can be suitable for use in the following method for manufacturing a semiconductor device (A).
[0088] Semiconductor device manufacturing method (A)
[0089] A method for manufacturing a semiconductor device comprising the following steps:
[0090] (a) a step of laminating a back-grinding substrate to the surface of the wafer on which the circuit pattern is formed;
[0091] (b) back grinding process, grinding the back side of the wafer;
[0092] (c) a step of attaching the adhesive tape of the present invention to the back side of the wafer and fixing it to a ring frame;
[0093] (d) a step of peeling the back-grinding substrate from the wafer;
[0094] (e) an adhesive film laminating step of fixing the adhesive tape of the present invention to which the wafer is laminated by vacuum adsorption from the substrate film side of the adhesive tape to a heated chuck stage, and laminating the adhesive film to the surface of the wafer opposite to the adhesive tape;
[0095] (f) a modified region forming step of irradiating a portion of the wafer to be divided with laser light from the adhesive tape side to form a modified region based on multiphoton absorption inside the wafer;
[0096] (g) an expansion step, in which the wafer and the adhesive film are cut along a cutting line by expanding the adhesive tape to obtain a plurality of wafer chips with an adhesive layer;
[0097] (h) a heat shrinking step of heating and shrinking the outer periphery of the portion of the adhesive tape where the wafer chips are arranged, thereby removing the slack generated in the above-mentioned expansion step and maintaining the interval between the chips;
[0098] (i) Picking up the wafer chip with the adhesive layer from the adhesive layer of the adhesive tape.
[0099] The present semiconductor device manufacturing method is a method using stealth dicing.
[0100] <How to use>
[0101] Reference Figure 2 to Figure 5 A method of using the adhesive tape 10 of the present invention when applied to the above-mentioned method (A) for producing a semiconductor device will be described.
[0102] First, a back grinding substrate is bonded to the surface of the wafer 30 having the circuit pattern 31 formed thereon (step (a)), and a back grinding step (step (b)) (not shown) of grinding the back side of the wafer 30 is performed. The back grinding substrate may be a common back grinding substrate, such as a glass substrate.
[0103] The adhesive tape 10 of the present invention is adhered to the back of the wafer 30 after the back grinding process is completed, and then bonded and fixed to the ring frame 20 (process (c)). At this time, the adhesive layer 12 of the adhesive tape 10 of the present invention is arranged in a manner of contacting the back of the wafer 30, and the ring frame 20 is arranged in the portion where the adhesive layer 12 is exposed around the wafer 30.
[0104] The back grinding substrate (not shown) is peeled off from the wafer 30 (step (d)).
[0105] like Figure 2 As shown, the adhesive tape 10 of the present invention with the wafer 30 bonded thereto is fixed to the heated chuck table 70 by vacuum adsorption from the base film 11 side, and the adhesive film 40 with a release film composed of the adhesive film 41 and the release film 42 is bonded to the surface of the wafer 30 (step e). In consideration of bonding with an adhesive film such as NCF, the heating temperature of the chuck table 70 at this time can be set to 80° C. or above.
[0106] The release film 42 is peeled off from the adhesive film 41. The state after the release film 42 is peeled off is shown in FIG. Figure 3 .
[0107] Then, if Figure 4 As shown, the wafer 30 to which the adhesive tape 10 is attached is unloaded from the chuck table 70. At this time, when an adhesive tape other than the adhesive tape of the present invention is used, the irregularities of the chuck table surface are transferred to the back surface of the base film 11, resulting in a state where the transmittance of the laser light is reduced. However, when the adhesive tape 10 of the present invention is used, this transfer can be effectively suppressed, and the transmittance of the laser light can be sufficiently maintained.
[0108] Then, if Figure 5 As shown in FIG. 1 , the laser beam 60 is irradiated from the adhesive tape 10 side toward the portion to be divided of the wafer 30, thereby forming a modified region 32 based on multiphoton absorption inside the wafer 30 (step (f)). Figure 5 In the embodiment, the reformed regions 32 are intermittently formed at four locations.
[0109] Next, the adhesive tape 10 of the present invention on which the wafer 30 and the ring frame 20 are bonded is placed on the table of the expansion device with the base film 11 side facing downward.
[0110] Next, while the annular frame 20 is fixed, the hollow cylindrical lifting member of the expansion device is raised to expand (expand) the adhesive tape 10 (process (g)). As expansion conditions, the expansion speed is, for example, 5 to 500 mm / second, and the expansion amount (lifting amount) is, for example, 5 to 25 mm. In this way, the adhesive tape 10 is stretched in the radial direction of the chip 30, and the chip 30 is cut into chip 33 units starting from the above-mentioned modified area 32. At this time, the elongation (deformation) caused by the expansion of the adhesive film 41 in the part bonded to the chip 30 is suppressed and does not break, but at the position between the chips 33, the tension caused by the expansion of the film is concentrated and breaks occur. Therefore, the adhesive film 41 is also cut together with the chip 30. As a result, Figure 6 As shown, a plurality of chips 33 with adhesive films 43 can be obtained.
[0111] Next, the following process is performed: the lifting member is returned to the original position, and the slack of the adhesive tape 10 generated in the previous expansion process is removed to stably maintain the interval between the chips 33. In this process, for example, a hot air nozzle is used to blow hot air at 40 to 120°C to the annular heating and shrinking area between the area where the chip 33 exists in the adhesive tape 10 and the annular frame 20 to heat and shrink the base film 11, so that the adhesive tape 10 is restored to a tense state (process (h)). Then, the adhesive layer 12 is subjected to energy ray curing treatment or heat curing treatment, etc., to weaken the adhesive force of the adhesive layer 12 on the chip 33, and then the chip 33 is picked up (process (i)).
[0112] Example
[0113] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0114] Use the following ingredients.
[0115] (Adhesive)
[0116] Base resin A: 2-methacryloyloxyethyl isocyanate was added to an acrylic copolymer (glass transition temperature: -65°C) having 70% by mass of 2-ethylhexyl acrylate, 29% by mass of 2-hydroxyethyl acrylate, and 1% by mass of methacrylic acid as structural units so that the double bond content was 0.9 (meq / g). 0.3 parts by mass of a urethane acrylate oligomer having a weight average molecular weight of 850 was added to 100 parts by mass of the acrylic copolymer as base resin A.
[0117] Photopolymerization initiator: Irgacure 184 (trade name, manufactured by Nippon Ciba Geigy)
[0118] Curing agent: Coronate L (isocyanate curing agent, trade name, manufactured by Tosoh Corporation)
[0119] Surface modifier: TEGORad2200N (trade name, manufactured by Tego Chemie)
[0120] (Base film)
[0121] EMMA: Ethylene-methyl methacrylate copolymer (AN4214C (trade name), manufactured by Dow-Mitsui Polychemicals Co., Ltd.)
[0122] ION (1): ionomer (Himilan 1855 (trade name), manufactured by Dow-Mitsui Polychemicals Co., Ltd.)
[0123] ION (2): ionomer (Himilan 1652 (trade name), manufactured by Dow-Mitsui Polychemicals Co., Ltd.)
[0124] ION (3): ionomer (Himilan AM7326 (trade name), manufactured by Dow-Mitsui Polychemicals Co., Ltd.)
[0125] PP: Polypropylene (F724P (trade name), manufactured by Prime Polymer Co., Ltd.)
[0126] <Example>
[0127] 1) Preparation of substrate film
[0128] (Base film 1)
[0129] EMMA was melt-kneaded and extruded at 220°C using a multilayer T-die extruder and extruded onto a metal roller (hereinafter referred to as "mirror roller (1)") with a single side mirror-finished. Thus, a substrate film 1 with a thickness of 100 μm was formed on the mirror roller (1). The surface shape of the metal roller was transferred to the mirror roller (1) side surface of the substrate film 1. The surface roughness Ra of the mirror roller (1) side surface of the obtained substrate film 1 was 0.03 μm.
[0130] (Base film 2)
[0131] In the preparation of the base film 1 , the base film 2 was prepared in the same manner as the base film 1 except that the mirror-finished roll ( 2 ) was used instead of the mirror-finished roll ( 1 ).
[0132] (Base film 3)
[0133] In the preparation of the base film 1 , a base film 3 was prepared in the same manner as the base film 1 , except that ION (3) was used instead of EMMA.
[0134] (Base film 4)
[0135] In the preparation of the base film 1, a base film 4 having a total thickness of 100 μm and including an ION (1) layer and an EMMA layer was prepared in the same manner as the base film 1, except that ION (1) and EMMA were co-extruded using a multilayer T-die extruder instead of EMMA so that EMMA was on the mirror roller (1) side. In the total amount of the resin component of the base film 4, ION (1) accounted for 50% by mass and EMMA accounted for 50% by mass. In addition, the thickness of the ION (1) layer was 50 μm, and the thickness of the EMMA layer was 50 μm.
[0136] (Base film 5)
[0137] In the preparation of the substrate film 4, the amounts of ION (1) and EMMA were such that ION (1) accounted for 20% by weight and the EMMA layer accounted for 80% by weight of the total amount of the resin components of the substrate film, and the substrate film 5 was prepared in the same manner as the substrate film 4. The thickness of the ION (1) layer was 20 μm, and the thickness of the EMMA layer was 80 μm.
[0138] (Base Film 6)
[0139] In the preparation of the base film 5, the base film 6 was prepared in the same manner as the base film 5 except that the total thickness was set to 150 μm. The thickness of the ION (1) layer was 30 μm, and the thickness of the EMMA layer was 120 μm.
[0140] (Base Film 7)
[0141] A base film 7 was prepared in the same manner as the base film 1 except that PP was used instead of EMMA in the preparation of the base film 1 .
[0142] (Base film 8)
[0143] In the preparation of the base film 1 , a base film 8 was prepared in the same manner as the base film 1 , except that ION (1) was used instead of EMMA.
[0144] (Base Film 9)
[0145] In the preparation of the base film 1 , a base film 9 was prepared in the same manner as the base film 1 , except that ION (2) was used instead of EMMA.
[0146] (Base Film 10)
[0147] In the preparation of the base film 1, a base film 10 having a total thickness of 100 μm and including an EMMA layer and an ION (1) layer was prepared in the same manner as the base film 1, except that EMMA and ION (1) were coextruded in place of EMMA so that ION (1) was on the mirror roller (1) side. Of the total amount of the resin component of the base film 10, EMMA accounted for 50% by mass and ION (1) accounted for 50% by mass. In addition, the thickness of the EMMA layer was 50 μm, and the thickness of the ION (1) layer was 50 μm.
[0148] (Base Film 11)
[0149] In the preparation of the base film 1 , a base film 11 was prepared in the same manner as the base film 1 except that the embossing roll ( 1 ) was used instead of the mirror roll ( 1 ).
[0150] (Base film 12)
[0151] In the preparation of the base film 1, a base film 12 was prepared in the same manner as the base film 1, except that the embossing roll (2) was used instead of the mirror roll (1).
[0152] 2) Preparation of adhesive composition
[0153] 3 parts by mass of a photopolymerization initiator, 1 part by mass of a curing agent, and 0.6 parts by mass of a surface modifier were mixed with 100 parts by mass of the base resin A. Thus, a pressure-sensitive adhesive composition having an acrylic resin as a base polymer was obtained.
[0154] 3) Preparation of adhesive tape
[0155] The adhesive composition obtained above was applied to a release liner composed of a polyethylene terephthalate film that had been subjected to a mold release treatment so that the thickness after drying was 20 μm, and dried at 110° C. for 3 minutes to obtain an adhesive film with a release liner. Next, the adhesive layer of the adhesive film with a release liner was attached to the surface of the substrate films 1 to 12 that was not in contact with the roller, and the release liner was peeled off, thereby obtaining adhesive tapes of Examples 1 to 6 and Comparative Examples 1 to 6 in which an adhesive layer was formed on the substrate films 1 to 12.
[0156] In this case, the arrangement of each layer constituting the base film of the base films 4 to 6 and 10 having a two-layer structure is as shown in Table 1.
[0157] The melting point, surface roughness Ra, and penetration temperature of each base film used in each pressure-sensitive adhesive tape of Examples and Comparative Examples were measured as follows.
[0158] (Melting point of base film)
[0159] The melting point of the base film was determined by measuring the melting peak temperature according to the DSC method (JIS K 7121: 2001), and the melting point was defined as the melting point. As the sample, each of the base films 1 to 12 obtained above was used.
[0160] When a plurality of melting peaks were confirmed, the temperature of the melting peak with the lowest temperature was taken as the melting point.
[0161] (Needle penetration temperature on the back side of the substrate film)
[0162] The pressure-sensitive adhesive layer of each pressure-sensitive adhesive tape obtained above was attached to a quartz base, and the back surface of the base film was measured.
[0163] The measurement was performed in accordance with JIS K7196: 2012, with a temperature increase rate of 5°C / min and a load of 500 mN applied to the tip of an indenter having a diameter of 1 mm. A TMA curve (horizontal axis: temperature, vertical axis: deformation) was obtained to determine the penetration temperature.
[0164] As a measuring apparatus, TMA8311 (trade name, manufactured by Rigaku Corporation) was used, and the measurement was performed in a needle penetration mode.
[0165] It should be noted that, for the substrate films 4 to 6 and 10 composed of multiple layers, the penetration temperature was also measured on the side (surface) of the substrate film on which the adhesive layer was formed. In this case, the adhesive layer was formed on the back side of the substrate film, and the adhesive tape was formed in the same manner as in the preparation of the adhesive tape 3) above, and the measurement was performed.
[0166] The needle penetration temperature (T2) at the back side of the substrate film is shown in the "Needle penetration temperature of substrate film" column of Table 1, and the difference ((T2)-(T1)) between the needle penetration temperature (T2) at the back side of the substrate film and the needle penetration temperature (T1) at the surface of the substrate film is shown in the "Needle penetration temperature difference (T2)-(T1) (°C)" column of Table 1. "-" means not measured.
[0167] (Surface roughness Ra of the back side of the substrate film)
[0168] Regarding the surface roughness Ra of the back side of the substrate film, the adhesive layer of each adhesive tape obtained above was adhered and fixed to a smooth silicon mirror wafer, and measured at any 5 locations (length about 5 mm × 5 locations) on the back side of the substrate film, and the average value was taken as the surface roughness Ra of the back side.
[0169] The measurement was performed using a measuring device: "Surftest SJ-310" (manufactured by Mitutoyo Co., Ltd.) JIS B0601. The measurement conditions were as follows.
[0170] -Measurement conditions-
[0171] Curve: R
[0172] Parameters: 2
[0173] Filter: Gaussian
[0174] λc: 0.8mm
[0175] λs: 2.5μm
[0176] Number of intervals: 5
[0177] (Yield point before 50% elongation when stretched at -15°C)
[0178] A stress-elongation curve at -15°C was obtained as follows, and the presence or absence of a yield point at an elongation of 50% (1.5 times the initial length) was confirmed.
[0179] Using a tensile test apparatus in accordance with JIS B7721:2018, the stress and elongation of each substrate film were measured by a tensile test under the following measurement conditions, and the stress-elongation curves were obtained using the results. The presence or absence of a yield point at an elongation of 50% (range of elongation 0 to 50%) was confirmed from the obtained stress-elongation curve. A test piece with a width of 5 mm (MD direction) and a length of 60 mm (TD direction) was cut from each substrate film as a test piece.
[0180] -Measurement conditions-
[0181] Measuring temperature: -15℃
[0182] The sample was placed in a low-temperature thermostatic bath, and the measurement was started 5 minutes after the temperature reached -15°C.
[0183] Distance between chucks: 20mm
[0184] Stretching speed 300mm / min
[0185] (stress)
[0186] A stress-elongation curve was prepared under the same measurement conditions as in the yield point test, and the stress value (MPa) at 30% elongation (elongation 30%) was determined. The following test pieces were used as test pieces.
[0187] Test piece A: Test piece with a width of 5 mm in the MD direction and a length of 60 mm in the TD direction
[0188] Test piece B: Test piece with a width of 5 mm in the TD direction and a length of 60 mm in the MD direction
[0189] The stress value of the test piece A is defined as the TD stress (S2), and the stress of the test piece B is defined as the MD stress (S1), and S1-S2 is calculated.
[0190] The transmittance after heat adsorption, meandering of the modified region during stealth dicing, tape breakage during cold expansion, and kerf width of each of the pressure-sensitive adhesive tapes of Examples and Comparative Examples were evaluated as follows.
[0191] (Transmittance after heating adsorption)
[0192] Each adhesive tape obtained in the embodiment and the comparative example is pasted on a ring frame (inner diameter: 350 mm). Then, each adhesive tape is placed on a porous chuck table (Porous Chuck (trade name), manufactured by Yoshioka Seiko Co., Ltd., material: alumina, 12-inch chip size, porous average pore size: 55 μm) heated to 80°C in a manner such that the back side (the side not coated with adhesive) becomes the chuck table side, and is adsorbed and fixed at a vacuum pressure of 90 kPa, and this state is maintained for 5 minutes. Then, each adhesive tape is removed from the chuck table, and light is irradiated from the back side of each adhesive tape, and the transmittance is measured using an ultraviolet visible spectrophotometer device (manufactured by Shimadzu Corporation, trade name: UV-1800). The measurement is performed at any 5 locations of each adhesive tape, and the average value of the transmittance at 650 nm is calculated as the transmittance after heating and adsorption.
[0193] Metering mode: %T
[0194] Scanning range: 1100~200nm
[0195] Recording range: 0.0~100.0%
[0196] Scanning speed: high speed
[0197] Scanning distance: Automatic
[0198] Scan times: 1
[0199] In the above test, the heating temperature of the chuck stage was set to 80° C., which is a temperature generally used when bonding an adhesive film to a wafer.
[0200] 650 nm is a typical wavelength of laser light provided in an autofocus unit for determining the processing depth of a modified region by laser irradiation in a cutting device.
[0201] (Meandering of modified area during stealth cutting)
[0202] 1) Invisible cutting
[0203] A silicon mirror wafer (diameter: 12 inches, thickness: 100 μm) and a ring frame are pasted to the adhesive layer of the adhesive tape to obtain a laminated structure. Similar to the above-mentioned transmittance test after heating and adsorption, the obtained laminated structure is fixed by adsorption from the back side of each adhesive tape (the side not coated with adhesive) with a vacuum pressure of 90 kPa using a porous chuck stage heated to 80°C, and this state is maintained for 5 minutes. Then, after the above-mentioned laminated structure is set in a laser slicer (manufactured by DISCO, product name "DF-7362"), the laminated structure is irradiated with a laser for stealth cutting from the back side of the adhesive tape to form modified areas at certain intervals in the silicon mirror wafer. More specifically, laser irradiation is performed in a manner that forms dot-shaped modified areas on a straight line along a predetermined line A in the cross section of the wafer chip obtained by stealth cutting. The width of the predetermined line A in the thickness direction of the wafer chip is about 0.1 mm / s. Figure 5 The length of the reformed region 32 in the thickness direction in the cross section of the wafer 30 shown is uniform. In this evaluation, the width of the predetermined line A is 20 μm.
[0204] Then, the above-mentioned stacked structure is placed in a chip dividing machine (manufactured by DISCO, product name "DDS2300"), and expanded (cold expanded) at -15°C with an expansion speed (pull-down speed) of 300 mm / sec and an expansion amount of 12 mm to obtain a 8mm×8mm chip. Then, it is further expanded at room temperature with an expansion speed of 5 mm / sec and an expansion amount of 10 mm. Then, heat shrink treatment is performed under the following conditions. Here, the expansion amount refers to the change in the relative position of the annular frame and the lifting member before and after pressing down. In this way, the wafer chip is obtained on the adhesive tape pasted on the annular frame by cold expansion cutting and heat shrinkage, and is picked up.
[0205] [condition]
[0206] Heater set temperature: 220℃
[0207] Hot air volume: 40L / min
[0208] The distance between the heater and the adhesive tape: 20 mm
[0209] Heater speed: 7° / sec
[0210] 2) The meandering of the modified area during stealth cutting
[0211] Use a digital microscope (manufactured by Keyence Corporation, VHX-5000 (trade name)) to observe the cross section (side formed by the above-mentioned cutting) (any one side) of the wafer chip obtained by the above-mentioned stealth cutting, and confirm the modified area of the wafer chip cross section. It was observed that the modified area in the cross section was spaced apart in a dotted manner in the length direction of the wafer chip. The width a1 of the rectangle containing the minimum area of all modified areas formed above the upper end in the thickness direction of the wafer chip of the predetermined line A in the cross section (the length in the thickness direction of the wafer chip) and the width a2 of the rectangle containing the minimum area of all modified areas formed below the lower end in the thickness direction of the wafer chip of the predetermined line A are measured, and the larger of a1 and a2 is used as the winding amount of the modified area in the cross section. If the winding amount is zero, the widths a1 and a2 of the rectangle are zero. The obtained winding amount is applied to the following evaluation levels for evaluation.
[0212] If the amount of meandering of the reformed region is large in the vertical direction of the thickness of the wafer chip, the chip may not be divided with good processing accuracy.
[0213] - Rating -
[0214] ◎: Less than 10μm
[0215] ○: 10 μm or more and less than 20 μm
[0216] △: 20μm or more and less than 30μm
[0217] ×: 30 μm or more
[0218] (Belt breakage during cold expansion)
[0219] The above-mentioned 1) invisible cutting was performed on 10 pieces of each adhesive tape. Whether the adhesive tape was broken during cold expansion was confirmed and evaluated according to the following evaluation levels.
[0220] If the adhesive tape breaks during cold expansion, the next step cannot be performed and the yield rate is deteriorated, which is not preferable.
[0221] - Rating -
[0222] ×: Any one of the 10 adhesive tapes was broken
[0223] 0: None of the 10 adhesive tapes broke
[0224] (Incision Width)
[0225] like Figure 7 As shown, the unnotched thickness of the adhesive tape in the MD direction is measured. Figure 7 The incision width X (MD incision width) between the rightmost chip 50a and the adjacent chip near the center in the MD direction, and the incision width Y (TD incision width) between the chip 50a and the adjacent chip near the center in the TD direction. Figure 7 The MD direction cut width and TD direction cut width are also measured for the leftmost chip 50b. In addition, the MD direction cut width and TD direction cut width are also measured for the chips 51 at the two ends without a notch in the TD direction of the adhesive tape and the chip 52 located in the center. The average value of the MD direction cut width and the average value of the TD direction cut width of the above five locations are calculated. The obtained cut width (μm) is applied to the following evaluation level for evaluation.
[0226] - Rating -
[0227] ◎: 30μm or more
[0228] 0: 20~29μm
[0229] △: 9~19μm
[0230] ×: 8 μm or less
[0231] The obtained results are summarized in Table 1 below.
[0232]
[0233] (Notes to Table 1)
[0234] The column "Rollers used in film formation" shows the rollers used in the production of each base film. "MR1" indicates a mirrored roller (1), "MR2" indicates a mirrored roller (2), "ER1" indicates an embossed roller (1), and "ER2" indicates an embossed roller (2).
[0235] The following can be seen from Table 1 above.
[0236] The pressure-sensitive adhesive tape of Comparative Example 1 has a base film made of PP having a high melting point (155° C.) The pressure-sensitive adhesive tape of Comparative Example 1 was broken during cold expansion.
[0237] The adhesive tapes of Comparative Examples 2 to 4 have a substrate film with a low needle penetration temperature on the back side of the substrate film. The adhesive tapes of Comparative Examples 2 to 4 all had a transmittance of less than 80% after vacuum adsorption on a chuck table under heating, and a meander of a modified region of more than 20 μm occurred during stealth dicing.
[0238] The adhesive tapes of Comparative Examples 5 and 6 have a substrate film with a large surface roughness Ra on the back of the substrate film. The transmittance after heat adsorption of the adhesive tapes of Comparative Examples 5 and 6 is less than 80%, and meandering of the modified area occurs during stealth cutting. Furthermore, the incision width becomes too narrow after heat shrinkage.
[0239] In contrast, the adhesive tapes of Examples 1 to 6 have a base film with a melting point of less than 150°C, a surface roughness Ra of less than 0.10 μm on the back, and a needle penetration temperature of more than 80°C. The transmittance of the adhesive tapes of Examples 1 to 6 after heating and adsorption is all above 84%, which allows the laser to fully penetrate, and the meandering of the modified area during stealth cutting is reduced to less than 20 μm. Furthermore, no fracture occurs during cold expansion. It can be seen that although the adhesive tape of the present invention uses a resin with a relatively low melting point, it shows sufficient transmittance to the laser after vacuum adsorption on the chuck table under heating, and has excellent expansion during expansion and cutting.
[0240] Furthermore, it was found that by using a base film having no yield point before 50% elongation in a stress-elongation curve at -15°C (Examples 3 to 6), the incision width can be appropriately maintained after heat shrinkage.
[0241] The present invention has been described in conjunction with its embodiments, but the applicant believes that, unless otherwise specified, the present invention is not limited to any details in the description and should be broadly interpreted without violating the spirit and scope of the invention as shown in the appended claims.
[0242] This application claims the priority based on Japanese Patent Application No. 2023-053186 filed in Japan on March 29, 2023, the contents of which are incorporated herein by reference as a part of the contents described in this specification.
[0243] Description of Reference Numerals
[0244] 10 Adhesive tape for cutting
[0245] 11. Base film
[0246] 12 Adhesive layer
[0247] 20 Ring frame
[0248] 30 chips
[0249] 31 Circuit surface
[0250] 32 Modified area
[0251] 33 Chip
[0252] 40 Adhesive film with release film
[0253] 41 Adhesive film
[0254] 42 peeling film
[0255] 60 Laser
[0256] 70 Chuck Table
Claims
1. A dicing adhesive tape comprising an adhesive layer on a substrate film, wherein: The melting point of the substrate film is 150° C. or lower, the surface A of the substrate film opposite to the adhesive layer has a surface roughness Ra of 0.10 μm or lower, and the penetration temperature of the surface A is 80° C. or higher.
2. The dicing adhesive tape according to claim 1, wherein The substrate film has no yield point before the elongation reaches 50% in a stress-elongation curve at -15°C.
3. The dicing adhesive tape according to claim 1 or 2, wherein: In a tensile test at -15°C, the absolute value of the difference between the stress S1 at 30% elongation in the MD direction, i.e., MD stress, and the stress S2 at 30% elongation in the TD direction, i.e., TD stress, is less than 4 MPa, wherein the unit of S1 is MPa.
4. The dicing adhesive tape according to any one of claims 1 to 3, wherein The base film is composed of at least two layers, and the relationship between the penetration temperature T1 of the surface on which the adhesive layer is formed and the penetration temperature T2 of the surface on which the adhesive layer is not formed satisfies [(T2)-(T1)]>0°C.
5. The dicing adhesive tape according to any one of claims 1 to 4, wherein The substrate film includes at least one of an ethylene-alkyl (meth)acrylate copolymer resin and an ionomer resin. 6 . The pressure-sensitive adhesive tape for dicing according to claim 1 , which is a stealth pressure-sensitive adhesive tape for dicing.