Antibacterial silk nanofiber composite hydrogel as well as preparation method and application thereof

Through the combination of polylysine-grafted silk nanofibers and porous hydrogel matrix, an antibacterial silk nanofiber composite hydrogel is formed, which solves the problem of insufficient antibacterial and biocompatibility of existing dressings and achieves efficient antibacterial Performance and wound healing support.

CN119055824APending Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411186707.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing wound dressings have shortcomings in antibacterial and biocompatible, leading to risk of bacterial growth and wound infection recurrence.

Method used

Polylysine-grafted silk nanofibers are used to combine with the porous hydrogel matrix to form an antibacterial silk nanofiber composite hydrogel, which serves as a support framework and filler, provides a three-dimensional network structure and porous structure to enhance the mechanics of the dressing Performance and antibacterial properties.

Benefits of technology

It achieves efficient antibacterial properties and good biocompatibility, keeps wound breathable, prevents bacterial growth, accelerates wound healing, and reduces the risk of wound adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014395120000131
    Figure BDA0005014395120000131
  • Figure HDA0005014395140000011
    Figure HDA0005014395140000011
  • Figure HDA0005014395140000012
    Figure HDA0005014395140000012
Patent Text Reader

Abstract

The invention discloses antibacterial silk nanofiber composite hydrogel as well as a preparation method and application thereof, and belongs to the technical field of biomedical materials. The antibacterial silk nanofiber composite hydrogel provided by the invention is prepared from polylysine grafted silk nanofibers and a hydrogel matrix. The wound dressing prepared from the antibacterial silk nanofiber composite hydrogel provided by the invention can keep the air permeability of the wound, avoid the breeding of bacteria, provide a wet environment, accelerate the healing of the wound and prevent the adhesion of the wound. The polylysine grafted silk nanofiber has a unique network structure and lasting antibacterial property, and the mechanical property and the antibacterial property of the antibacterial silk nanofiber composite hydrogel can be effectively adjusted by controlling the proportion and the dispersion state of the polylysine grafted silk nanofiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials, and particularly relates to an antibacterial silk nanofiber composite hydrogel and a preparation method and application thereof. Background Art

[0002] Hydrogel is a highly hydrated polymer material that ensures its structural integrity through physical and chemical interactions between molecules. It can swell and retain a large amount of water, but is insoluble in water. It can be used as an interactive wound dressing to absorb moisture or body fluids exuded from the wound, and can also isolate the wound to prevent bacterial infection in the air. In the prior art, in order to improve the antibacterial properties of dressings, common methods include adding antibiotics or metal ions with bactericidal effects to the dressings, and grafting antibacterial drugs onto the raw materials. The disadvantage of adding antibiotics or bactericidal drugs to the dressings is that the release rate of the drugs in the dressings is unstable. Therefore, grafting antibacterial drugs on dressings to improve the antibacterial ability of dressings is a widely studied and effective method in this field.

[0003] The Chinese patent with publication number CN114835917A provides a preparation method of regenerated silk fibroin / ε-polylysine composite hydrogel, its products and applications. The patent discloses the use of regenerated silk fibroin and ε-polylysine, EDC / NHS as a cross-linking agent to obtain a regenerated silk fibroin / ε-polylysine composite hydrogel, the maximum strength of which is about 3.8kPa, and the equilibrium swelling degree can exceed 400%. The hydrogel has a significant inhibitory effect on Staphylococcus aureus and Escherichia coli, and can be used as a wound repair material. However, the composite hydrogel disclosed in the patent does not use biocompatible macromolecular chitosan, chondroitin sulfate, sodium alginate, hyaluronic acid, collagen and gelatin to form a cross-linked hydrogel, so the composite hydrogel obtained in the patent has poor biocompatibility and no loose porous structure. It is directly used as a wound dressing, which is not conducive to wound ventilation, and is prone to bacterial growth, and there is a risk of recurrence of wound infection. Summary of the invention

[0004] In view of this, the object of the present invention is to provide an antibacterial silk nanofiber composite hydrogel and a preparation method and application thereof. The antibacterial silk nanofiber composite hydrogel provided by the present invention has good mechanical properties, antibacterial properties and biocompatibility as a dressing.

[0005] To solve the above problems, the specific implementation scheme of the present invention is as follows:

[0006] The present invention provides an antibacterial silk nanofiber composite hydrogel, comprising the following components: polylysine-grafted silk nanofibers, a hydrogel matrix and water;

[0007] The mass ratio of the polylysine grafted silk nanofibers to the hydrogel matrix is ​​1:2-49;

[0008] The mass content of water in the antibacterial silk nanofiber composite hydrogel is 45-95%;

[0009] The polylysine grafted silk nanofibers are a supporting skeleton; the polylysine grafted silk nanofibers present a three-dimensional network structure;

[0010] The hydrogel matrix is ​​a porous structure; the hydrogel matrix is ​​wrapped on the polylysine grafted silk nanofibers and filled in the pores of the polylysine grafted silk nanofibers;

[0011] The polylysine grafted silk nanofiber is ε-polylysine grafted silk nanofiber.

[0012] Preferably, the content of ε-polylysine in the polylysine-grafted silk nanofibers is 0-20wt%, and the content is not zero.

[0013] Preferably, the hydrogel matrix comprises one or more of chitosan, chondroitin sulfate, sodium alginate, hyaluronic acid, collagen and gelatin.

[0014] Preferably, the porosity of the antibacterial silk nanofiber composite hydrogel is 50-90%; the equilibrium water absorption rate is 500-1000%; the equilibrium swelling rate is 350-1500%; the compressive strength is 0.25-0.5 MPa; and the antibacterial rate is greater than 90%.

[0015] The present invention also provides a method for preparing the antibacterial silk nanofiber composite hydrogel described in the above technical solution, comprising the following steps:

[0016] The poly-lysine grafted silk nanofibers, the hydrogel matrix and water are mixed to obtain a hydrogel precursor;

[0017] A cross-linking agent is added to the hydrogel precursor to carry out a cross-linking reaction to obtain the antibacterial silk nanofiber composite hydrogel.

[0018] Preferably, the concentration of the hydrogel precursor is 2-10 wt %.

[0019] Preferably, the cross-linking agent comprises one or more of glutaraldehyde, glyoxal, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system, genipin, hydrogen peroxide and horseradish peroxidase system, laccase, tyrosinase, methanol, ethanol and calcium chloride;

[0020] The mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to N-hydroxysuccinimide in the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system is 1:0.2-1;

[0021] The mass of the cross-linking agent is 0.1-30% of the mass of the hydrogel precursor.

[0022] Preferably, the cross-linking reaction is carried out at a temperature of -25 to 60°C and for a time of 1 to 48 hours.

[0023] The present invention also provides the use of the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method in the preparation of wound dressings.

[0024] Preferably, the wound dressing is one of an antibacterial silk nanofiber composite hydrogel dressing and an antibacterial silk nanofiber composite hydrogel modified textile-based dressing;

[0025] The antibacterial silk nanofiber composite hydrogel dressing is made of the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method;

[0026] The antibacterial silk nanofiber composite hydrogel modified textile-based dressing comprises a hydrogel functional layer and a textile structure substrate layer; the hydrogel functional layer is loaded on the textile structure substrate layer; the thickness of the hydrogel functional layer is 0.5 to 5 mm; the textile structure substrate layer comprises one of medical absorbent cotton gauze, elastic bandage gauze, wound gauze, non-woven gauze and composite non-woven gauze;

[0027] The hydrogel in the hydrogel functional layer is the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method.

[0028] The invention provides an antibacterial silk nanofiber composite hydrogel, comprising the following components: polylysine grafted silk nanofiber, a hydrogel matrix and water; the mass ratio of the polylysine grafted silk nanofiber to the hydrogel matrix is ​​1:2-49; the mass content of water in the antibacterial silk nanofiber composite hydrogel is 45-95%; the polylysine grafted silk nanofiber is a supporting skeleton; the polylysine grafted silk nanofiber presents a three-dimensional network structure; the hydrogel matrix is ​​a porous structure; the hydrogel matrix is ​​wrapped on the polylysine grafted silk nanofiber and filled in the pores of the polylysine grafted silk nanofiber; the polylysine grafted silk nanofiber is ε-polylysine grafted silk nanofiber.

[0029] The antibacterial silk nanofiber composite hydrogel provided by the present invention presents a porous structure, and is directly or combined with a textile structure substrate layer to form a wound dressing, which can keep the wound breathable and avoid the breeding of bacteria, and at the same time can provide a moist environment, accelerate wound healing, and prevent wound adhesion. The polylysine-grafted silk nanofiber has a unique network structure and lasting antibacterial properties. By controlling the proportion of the polylysine-grafted silk nanofiber and its dispersion state, the mechanical properties and antibacterial properties of the antibacterial silk nanofiber composite hydrogel can be effectively adjusted. The present invention adopts ε-polylysine-grafted silk nanofiber as a supporting skeleton, which, on the one hand, ensures that the antibacterial silk nanofiber composite hydrogel has sufficient mechanical properties, and on the other hand, the ε-polylysine-grafted silk nanofiber has an inhibitory effect on fungi, Gram-positive bacteria, and Gram-negative bacteria, and has the advantages of high efficiency, safety, broad-spectrum antibacterial, and good stability. The present invention adopts ε-polylysine grafted silk nanofibers to replace the addition of antibiotics or bactericidal drugs in the dressing in the prior art, ensuring that the antibacterial silk nanofiber composite hydrogel has a lasting and balanced antibacterial property, while also overcoming the threats of drug resistance and biological toxicity. The antibacterial silk nanofiber composite hydrogel provided by the present invention has good antibacterial properties and biocompatibility, and has good application prospects as a wound dressing.

[0030] The results of the embodiments show that the porosity of the antibacterial silk nanofiber composite hydrogel prepared by the present invention is 50-90%; the equilibrium water absorption rate is 500-1000%; the equilibrium swelling rate is 350-1500%; the compressive strength is 0.25-0.5MPa, and it has good mechanical properties; the antibacterial rate is >90%.

[0031] The present invention also provides a method for preparing the antibacterial silk nanofiber composite hydrogel, comprising the following steps: mixing polylysine grafted silk nanofibers, a hydrogel matrix and water to obtain a hydrogel precursor; adding a crosslinking agent to the hydrogel precursor to perform a crosslinking reaction to obtain the antibacterial silk nanofiber composite hydrogel.

[0032] The present invention cross-links polylysine-grafted silk nanofibers with a hydrogel matrix to prepare an antibacterial silk nanofiber composite hydrogel. 1) The antibacterial properties of the antibacterial silk nanofiber composite hydrogel are improved by grafting antibacterial ε-polylysine on the silk nanofibers; 2) the antibacterial silk nanofibers are bent and intertwined, and as a mesh support skeleton, the mechanical properties of the antibacterial silk nanofiber composite hydrogel are improved; 3) more amino groups are added to the molecular chain of the silk nanofiber grafted polylysine, which is easy to react with the hydrogel matrix to form a gel by chemical cross-linking. The preparation method provided by the present invention has a controllable process, mild reaction and no toxicity, low raw material cost, wide source, and is conducive to large-scale standard production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1This is a SEM image of the poly-lysine grafted silk nanofibers prepared in Example 1;

[0034] Figure 2 This is a diameter distribution diagram of the polylysine grafted silk nanofibers prepared in Example 1;

[0035] Figure 3 This is a physical picture of the antibacterial silk nanofiber composite hydrogel prepared in Example 1;

[0036] Figure 4 This is the SEM image of the antibacterial silk nanofiber composite hydrogel prepared in Example 1. DETAILED DESCRIPTION

[0037] The present invention provides an antibacterial silk nanofiber composite hydrogel, comprising the following components: polylysine-grafted silk nanofibers, a hydrogel matrix and water;

[0038] The mass ratio of the polylysine grafted silk nanofibers to the hydrogel matrix is ​​1:2-49;

[0039] The mass content of water in the antibacterial silk nanofiber composite hydrogel is 45-95%;

[0040] The polylysine grafted silk nanofibers are a supporting skeleton; the polylysine grafted silk nanofibers present a three-dimensional network structure;

[0041] The hydrogel matrix is ​​a porous structure; the hydrogel matrix is ​​wrapped on the polylysine grafted silk nanofibers and filled in the pores of the polylysine grafted silk nanofibers;

[0042] The polylysine grafted silk nanofiber is ε-polylysine grafted silk nanofiber.

[0043] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0044] In the present invention, the porosity of the antibacterial silk nanofiber composite hydrogel is preferably 50-90%, more preferably 55-85%, and further preferably 55-80%. In the present invention, the equilibrium water absorption rate of the antibacterial silk nanofiber composite hydrogel is preferably 500-1000%, more preferably 800-1000%, and further preferably 800-950%; the equilibrium swelling rate is preferably 350-1500%, more preferably 600-1100%, and further preferably 750-1100%; the compressive strength is preferably 0.25-0.5MPa, and more preferably 0.3-0.5MPa; the antibacterial rate is >90%.

[0045] The antibacterial silk nanofiber composite hydrogel provided by the present invention comprises polylysine grafted silk nanofibers. In the present invention, the polylysine grafted silk nanofibers are the supporting skeleton, and the polylysine grafted silk nanofibers are in a three-dimensional network structure (such as Figure 1 In the present invention, the polylysine grafted silk nanofiber is an ε-polylysine grafted silk nanofiber. In the present invention, the ε-polylysine content in the polylysine grafted silk nanofiber is preferably 0 to 20 wt %, and the content is not 0, and more preferably 5 to 15 wt %.

[0046] In the present invention, the preparation method of the polylysine grafted silk nanofiber preferably includes the following steps: mixing silk nanofibers, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, N-hydroxysuccinimide and ε-polylysine, and performing a grafting reaction to obtain polylysine grafted silk nanofibers.

[0047] In the present invention, the diameter of the silk nanofiber is preferably <1000nm, more preferably 20-500nm, and further preferably 30-300nm. In the present invention, the silk nanofiber is preferably prepared into a suspension for use, and the concentration of the silk nanofiber in the suspension is preferably 0.5-10wt%, more preferably 0.5-4wt%. In the present invention, the method of preparing the suspension is preferably ultrasonic method, and the ultrasonic time is preferably 5-30min. In the present invention, silk nanofiber has good biocompatibility and mechanical properties. Due to its slow degradation in the body, it can be used for the attachment and proliferation of many cells, but the material has poor crystallinity and poor cell adhesion. In order to improve these problems, natural silk is prepared into a silk nanofiber suspension, and ε-polylysine is grafted on it, and it is compounded with other natural polymer materials to improve its antibacterial properties.

[0048] In the present invention, the molecular weight of the ε-polylysine is preferably <5000Da, more preferably 2000-5000Da. In the present invention, the ε-polylysine is preferably prepared into an ε-polylysine aqueous solution, and the concentration of the ε-polylysine aqueous solution is preferably 0.5-5wt%. In the present invention, the mass ratio of the silk nanofiber to the ε-polylysine is preferably 1:0-0.2, and is not 0, and more preferably 1:0.005-0.15. In the present invention, ε-polylysine (ε-PLL) is produced by fermentation of Streptomyces albus, which is completely non-toxic and edible. At the same time, ε-polylysine is composed of essential amino acids for the human body and can be biodegraded into lysine after digestion; in addition, the positively charged ε-polylysine has a wide antibacterial spectrum, and has an inhibitory effect on fungi, Gram-positive bacteria, and Gram-negative bacteria. It can be aggregated on the surface of negatively charged bacterial cell membranes, and electrostatic interactions occur with the bacterial surface, resulting in enhanced bacterial cell membrane permeability, destruction of the integrity of bacterial cell membranes, increased reactive oxygen content, and mediated antibacterial effects. Compared with traditional antibacterial drugs, ε-PLL is not easy to develop drug resistance, and in the inflammatory stage of wound healing, it can upregulate the expression of anti-inflammatory factors and regulate the body's immune function; in the proliferative stage, it can promote granulation tissue and angiogenesis, and promote wound healing.

[0049] In the present invention, the amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide added is preferably 2-10wt% of the mass of the silk nanofiber, and more preferably 5-7wt%. In the present invention, the amount of N-hydroxysuccinimide added is preferably 1-5wt% of the mass of the silk nanofiber, and more preferably 2.5-3.5wt%. In the present invention, the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to N-hydroxysuccinimide is 1:0.2-1.0.

[0050] In the present invention, the conditions of the grafting reaction are: reaction temperature 0 to 10°C, more preferably 0 to 5°C, further preferably 4°C, time is preferably 2 to 8h, more preferably 4 to 8h, further preferably 5h. In a specific embodiment of the present invention, the grafting reaction comprises: adding crosslinking agents 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide to the silk nanofiber suspension, stirring and mixing; then adding ε-polylysine aqueous solution to carry out grafting reaction. In the present invention, the grafting reaction is preferably carried out under the condition of magnetic stirring. In the present invention, the stirring time is preferably 4 to 8h.

[0051] In the present invention, after the grafting reaction, it is preferred that the reaction liquid is dialyzed and freeze-dried in sequence. In the present invention, the dialysis is preferably carried out in a dialysis bag. In the present invention, the temperature of the dialysis is preferably 0 to 10°C, more preferably 0 to 8°C, and further preferably 4 to 8°C. In the present invention, the dialysis time is preferably 2 to 3 days. In the present invention, the dialysis bag preferably has a molecular weight cutoff of >5000Da. In the present invention, the freeze-drying is preferably carried out in a freeze dryer. In the present invention, the freeze-drying temperature is preferably -50 to -40°C, more preferably -45 to -40°C, and the time is preferably 12 to 48h, more preferably 18 to 24h. In the present invention, it is preferred that the dialyzed product is pre-frozen first and then placed in a freeze dryer for freeze drying. In the present invention, the pre-freezing temperature is preferably -80 to -18°C, more preferably -30 to -20°C, and the pre-freezing time is preferably 8 to 24h, more preferably 12 to 24h. After the dialysis and freeze-drying, the poly-lysine grafted silk nanofibers are obtained.

[0052] The present invention uses 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide as crosslinking agents to graft ε-polylysine onto silk nanofibers. The present invention uses a 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide solution and an N-hydroxysuccinimide solution crosslinking system to graft polylysine onto nanofibers. As the grafting rate increases, the antibacterial properties of the antibacterial silk nanofiber composite hydrogel will be better, the fiber entanglement ability will increase, and the mechanical strength can be improved. However, when the proportion of ε-polylysine in silk nanofibers is too large (more than 20wt%), ε-polylysine is not easy to graft onto silk nanofibers. The present invention controls the molecular weight of ε-polylysine, as well as the mass ratio with silk nanofibers, and controls the grafting temperature at 0 to 10°C, so that the content of ε-polylysine in polylysine grafted silk nanofibers is preferably controlled at 0 to 20wt%, and the grafting rate is preferably not zero. The porosity of the antibacterial silk nanofiber composite hydrogel in the present invention is 50-90%, which ensures the mechanical properties of the polylysine grafted silk nanofiber as a supporting skeleton, while giving the antibacterial silk nanofiber composite hydrogel a loose porous structure to ensure biocompatibility and antibacterial properties. The polylysine grafted silk nanofiber prepared by the present invention has the advantages of a unique network structure and long-lasting antibacterial properties.

[0053] The present invention adopts polylysine grafted silk nanofibers with a three-dimensional network structure as a supporting skeleton. The polylysine grafted silk nanofibers have a unique network structure and lasting antibacterial properties. By controlling the proportion of polylysine grafted silk nanofibers and their loading content, the mechanical properties and antibacterial properties of the antibacterial silk nanofiber composite hydrogel can be effectively adjusted.

[0054] The antibacterial silk nanofiber composite hydrogel provided by the present invention includes a hydrogel matrix. In the present invention, the mass ratio of the polylysine grafted silk nanofiber to the hydrogel matrix is ​​1:2 to 49, preferably 1:4 to 19. In the present invention, the hydrogel matrix is ​​a porous structure, and the hydrogel matrix is ​​wrapped on the polylysine grafted silk nanofiber and filled in the pores of the polylysine grafted silk nanofiber.

[0055] In the present invention, the hydrogel matrix preferably includes one or more of chitosan, chondroitin sulfate, sodium alginate, hyaluronic acid, collagen and gelatin, more preferably one or more of gelatin, hyaluronic acid, sodium alginate, chitosan and collagen, and further preferably one or more of gelatin, hyaluronic acid, sodium alginate and chitosan. In the present invention, the hydrogel matrix presents a porous structure and is made into a wound dressing, which can keep the wound breathable and avoid bacterial growth. At the same time, it can provide a moist environment, accelerate wound healing, prevent wound adhesion, promote nutrient exchange, and have good biocompatibility.

[0056] The antibacterial silk nanofiber composite hydrogel provided by the present invention also includes water. In the present invention, the mass content of water in the antibacterial silk nanofiber composite hydrogel is 45-95%, preferably 55-90%. The water is preferably ultrapure water, deionized water or distilled water, more preferably deionized water or ultrapure water. In the present invention, the water content in the antibacterial silk nanofiber composite hydrogel can be adjusted according to actual needs, such as the water content can be reduced during low-temperature storage, and the water content can be increased during use. In the present invention, the specific adjustment method for increasing the water content is preferably to soak the antibacterial silk nanofiber composite hydrogel in water; the specific adjustment method for reducing the water content is preferably low-temperature freeze-drying, and the temperature is preferably -45 to -25°C. In the present invention, the hydrogel matrix with a porous structure can absorb and store more water, and the polylysine-grafted silk nanofiber as a supporting skeleton is also hydrophilic, which can allow the antibacterial silk nanofiber composite hydrogel to retain water for a long time, which is beneficial to wound healing. The water content of the antibacterial silk nanofiber composite hydrogel provided by the present invention is ≥45%, and the biological activity and use performance of the antibacterial silk nanofiber composite hydrogel can be maintained.

[0057] The present invention provides a method for preparing the antibacterial silk nanofiber composite hydrogel described in the above technical solution, comprising the following steps:

[0058] The poly-lysine grafted silk nanofibers, the hydrogel matrix and water are mixed to obtain a hydrogel precursor;

[0059] A cross-linking agent is added to the hydrogel precursor to carry out a cross-linking reaction to obtain the antibacterial silk nanofiber composite hydrogel.

[0060] The invention mixes polylysine grafted silk nanofibers, a hydrogel matrix and water to obtain a hydrogel precursor.

[0061] In the present invention, the polylysine grafted silk nanofibers are preferably formulated into a polylysine grafted silk nanofiber suspension, and the concentration of the polylysine grafted silk nanofiber suspension is preferably 1 to 10wt%. In the present invention, the hydrogel matrix is ​​preferably formulated into a hydrogel matrix solution. In a specific embodiment of the present invention, it preferably includes a chitosan solution, a sodium alginate solution, a hyaluronic acid solution, a collagen solution or a gelatin solution. In the present invention, the concentration of the hydrogel matrix solution is preferably 1 to 10wt%. In the present invention, the solvent in the polylysine grafted silk nanofiber suspension and the hydrogel matrix solution is preferably water, more preferably ultrapure water, deionized water or distilled water, and further preferably deionized water.

[0062] After obtaining the hydrogel precursor, the present invention adds a crosslinking agent to the hydrogel precursor to carry out a crosslinking reaction to obtain the antibacterial silk nanofiber composite hydrogel.

[0063] In the present invention, the concentration of the hydrogel precursor is 2-10wt%, preferably 3-8wt%. In the present invention, the concentration of the hydrogel precursor refers to the concentration of the total mass of the polylysine grafted silk nanofibers and the hydrogel matrix in the hydrogel precursor.

[0064] In the present invention, the cross-linking agent preferably includes one or more of glutaraldehyde, glyoxal, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system, genipin, hydrogen peroxide and horseradish peroxidase system, laccase, tyrosinase, methanol, ethanol and calcium chloride, and more preferably one or more of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system, genipin, hydrogen peroxide and horseradish peroxidase system, tyrosinase and calcium chloride. In the present invention, the mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to N-hydroxysuccinimide in the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system is preferably 1:0.2 to 1, and more preferably 1:0.5 to 1. In the present invention, the ratio of hydrogen peroxide to horseradish peroxidase in the hydrogen peroxide and horseradish peroxidase system is preferably 0.05-0.3 mmol: 200-800 u.

[0065] In the present invention, the mass of the cross-linking agent is preferably 0.1-30% of the mass of the hydrogel precursor, more preferably 0.1-20%, further preferably 0.1-10%, and further preferably 0.1-8%. In the present invention, the cross-linking agent is preferably formulated into an aqueous solution for use, and the concentration of the cross-linking agent solution is preferably 0-50 mg / mL, and the concentration is not 0, more preferably 1-20 mg / mL, and further preferably 2-10 mg / mL. In the present invention, the cross-linking agent stimulates the cross-linking of polylysine grafted silk nanofibers and the hydrogel matrix to form a composite network structure. In the present invention, the amount of the cross-linking agent is closely related to the type of the cross-linking agent, so the amount of the cross-linking agent is not included in the calculation of the mass ratio of each component in the antibacterial silk nanofiber composite hydrogel.

[0066] In the present invention, the temperature of the cross-linking reaction is preferably -25 to 60°C, the time is preferably 1 to 48 hours, more preferably 3 to 24 hours, and further preferably 3 to 18 hours. In a specific embodiment of the present invention, the cross-linking reaction preferably includes room temperature cross-linking and freeze-thaw cross-linking. In the present invention, the conditions for room temperature cross-linking are preferably: reaction temperature 20 to 60°C, more preferably 20 to 45°C, reaction time is preferably 1 to 48 hours, more preferably 3 to 24 hours. In the present invention, the conditions for freeze-thaw cross-linking are preferably: stirring at 20 to 50°C for 1 to 3 hours, then freezing the reaction liquid at -25 to -18°C for 12 to 24 hours, and finally thawing at 15 to 30°C for 2 to 8 hours.

[0067] The present invention also provides the use of the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method in the preparation of wound dressings.

[0068] In the present invention, the wound dressing is preferably one of an antibacterial silk nanofiber composite hydrogel dressing and an antibacterial silk nanofiber composite hydrogel modified textile-based dressing.

[0069] In the present invention, the antibacterial silk nanofiber composite hydrogel dressing is preferably made of the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method.

[0070] In the present invention, the antibacterial silk nanofiber composite hydrogel modified textile-based dressing preferably includes a hydrogel functional layer and a textile structure substrate layer. In the present invention, the hydrogel functional layer is loaded on the textile structure substrate layer. In the present invention, the thickness of the hydrogel functional layer is preferably 0.5 to 5 mm, more preferably 1 to 3 mm. In the present invention, the textile structure substrate layer preferably includes one of medical absorbent cotton gauze, elastic bandage gauze, wound gauze, non-woven gauze and composite non-woven gauze. In the present invention, the hydrogel in the hydrogel functional layer is preferably the antibacterial silk nanofiber composite hydrogel described in the above technical solution or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method.

[0071] The antibacterial silk nanofiber composite hydrogel prepared by the present invention has excellent biocompatibility and antibacterial properties, and the dressing prepared directly or in combination with a textile structure substrate layer can be used for treating different types of wounds, and has considerable application prospects. The textile structure substrate layer used in the present invention is all natural material, safe, non-toxic, economical and easy to obtain.

[0072] The technical solution of the present invention is further illustrated by specific implementation methods below. Those skilled in the art should understand that the embodiments described below are only part of the embodiments of the present invention, which are used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0073] Example 1

[0074] (1) Preparation of polylysine grafted silk nanofibers:

[0075] 0.3g of silk nanofibers, 0.015g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, 0.0075g of N-hydroxysuccinimide and 0.015g of ε-polylysine were mixed and subjected to grafting reaction at 4°C for 5h to obtain a reaction solution. The reaction solution was transferred into a dialysis bag and dialyzed at 4°C for 2 days to retain products with a molecular weight of >5000Da. The product obtained after dialysis was pre-frozen at -20°C for 8h, and then the pre-frozen product was transferred into a freeze dryer and freeze-dried at -40°C for 24h to obtain polylysine-grafted silk nanofibers.

[0076] Figure 1 This is the SEM image of the polylysine grafted silk nanofibers prepared in Example 1. Figure 1 It can be seen that the polylysine grafted silk nanofibers prepared by the present invention have uniform diameters, are interlaced with each other, and present a three-dimensional network structure. Many holes are distributed between the polylysine grafted silk nanofibers, which serve as a supporting skeleton to ensure mechanical strength while having good air permeability.

[0077] Figure 2The diameter distribution diagram of the polylysine grafted silk nanofibers prepared in Example 1 is shown in FIG. Figure 2 It can be seen that the diameter of polylysine grafted silk nanofibers is distributed between 20 and 140 nm, and the diameter between 80 and 100 nm accounts for the highest proportion. It has the advantages of large specific surface area and uniform diameter distribution, which is conducive to composite with hydrogel matrix.

[0078] (2) Preparation of antibacterial silk nanofiber composite hydrogel:

[0079] After evenly mixing 5 mL of 3 wt% poly-lysine grafted silk nanofiber suspension and 10 mL of 7 wt% gelatin solution, 2 mL of 5 mg / mL genipin solution was added. After stirring at 50 °C for 1 h, the reaction liquid was frozen at -18 °C for 24 h, and then thawed at 20 °C for 4 h to obtain an antibacterial silk nanofiber composite hydrogel.

[0080] In this embodiment, genipin is used as a cross-linking agent, so that the poly-lysine grafted silk nanofibers and the gelatin solution can be freeze-thaw cross-linked to form a hydrogel.

[0081] Figure 3 This is a physical picture of the antibacterial silk nanofiber composite hydrogel prepared in Example 1. Figure 3 It can be seen that the antibacterial silk nanofiber composite hydrogel is well formed, has a uniform texture, no stratification, no turbidity, and presents a certain degree of transparency, which proves that the polylysine grafted silk nanofibers are well blended with the hydrogel matrix; and the antibacterial silk nanofiber composite hydrogel does not drool after being inverted, which proves that the antibacterial silk nanofiber composite hydrogel prepared by the present invention has good mechanical strength and has long-lasting water retention properties while providing a humid environment.

[0082] Figure 4 This is the SEM image of the antibacterial silk nanofiber composite hydrogel prepared in Example 1. Figure 4 It can be seen that the surface of the antibacterial silk nanofiber composite hydrogel is dense, and it can be observed that the polylysine grafted silk nanofibers are successfully loaded in the hydrogel matrix. The polylysine grafted silk nanofibers are evenly distributed in the hydrogel matrix, which can ensure that the antibacterial silk nanofiber composite hydrogel has good mechanical strength; and there are many holes inside the antibacterial silk nanofiber composite hydrogel. As a wound dressing, it keeps the wound breathable and has lasting antibacterial properties. It can also absorb moisture to provide a moist environment, which is conducive to accelerated wound healing.

[0083] Example 2

[0084] 7 mL of 1 wt% poly-lysine grafted silk nanofiber suspension and 5 mL of 3 wt% hyaluronic acid solution were stirred evenly, and then 0.15 mmol of hydrogen peroxide and 600 u of horseradish peroxidase were added. After stirring evenly, the mixture was poured into a mold and subjected to cross-linking reaction at 37°C for 12 hours to obtain an antibacterial silk nanofiber composite hydrogel.

[0085] In this embodiment, hydrogen peroxide and horseradish peroxidase system are used to catalyze the cross-linking reaction between polylysine grafted silk nanofibers and hyaluronic acid, which has the characteristics of fast reaction speed, high cross-linking degree and no toxic side effects.

[0086] Example 3

[0087] 5 mL of 2 wt% poly-lysine grafted silk nanofiber suspension was evenly stirred with 10 mL of 5 wt% sodium alginate solution, and then 2 mL of 5.55 mg / mL calcium chloride solution was added. After stirring evenly, the mixture was poured into a mold and cross-linked at room temperature of 25°C for 12 hours to obtain an antibacterial silk nanofiber composite hydrogel.

[0088] Example 4

[0089] After stirring evenly 10 mL of 3 wt% poly-lysine grafted silk nanofiber suspension and 10 mL of 3 wt% chitosan solution, 4 mL of 30 mg / mL 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide solution and 3 mL of 30 mg / mL N-hydroxysuccinimide solution were added, the mixture was quickly stirred evenly, poured into a mold, and placed at room temperature 25°C for cross-linking reaction for 12 hours to obtain an antibacterial silk nanofiber composite hydrogel.

[0090] Comparative Example 1

[0091] To 10 mL of 7 wt % gelatin solution, add 2 mL of 5 mg / mL genipin solution, stir at 50 ° C for 1 hour, transfer the reaction liquid mixture to a 15 ml tube, freeze it at -18 ° C for 24 hours, and then thaw it at 20 ° C for 4 hours to obtain gelatin hydrogel.

[0092] The water absorption rate of the antibacterial silk nanofiber composite hydrogel obtained in Examples 1 to 4 and Comparative Example 1 was detected by the following method. The water absorption rate testing method includes: placing the prepared antibacterial silk nanofiber composite hydrogel sample in deionized water, allowing it to absorb water and swell to a constant weight, weighing and recording the weight W of the sample s Next, the sample was placed in a -18°C refrigerator for 12 h and then freeze-dried for 48 h to obtain a completely dry antibacterial silk nanofiber composite hydrogel sample. The dry weight of the sample was weighed and recorded. d, three parallel experiments were performed, and the average value was taken to calculate the water absorption rate (W) of the hydrogel according to the following formula 1 吸水 ):

[0093] W 吸水 =(W s -W d ) / W s ×100%, in formula 1, W s and W d They are the weight of the antibacterial silk nanofiber composite hydrogel sample when it absorbs water to reach equilibrium and the weight when it is completely dry (g), respectively.

[0094] The swelling rate of the antibacterial silk nanofiber composite hydrogel obtained in Examples 1 to 4 and Comparative Example 1 was detected by the following method. The swelling rate testing method includes: freezing the antibacterial silk nanofiber composite hydrogel sample at -18°C for 12 hours, and then freeze-drying it for 48 hours to obtain a completely dried sample and weighing it, which is recorded as W. d Then, the sample was immediately immersed in PBS buffer solution (pH=7.4) for swelling test. The sample was taken out every 5 minutes and the excess water on its surface was wiped off with filter paper and weighed until the sample weight no longer changed, that is, the swelling equilibrium was reached. The weight was weighed and recorded as W. w Three parallel experiments were performed for each sample, and the average value was taken to calculate the swelling rate (W) of the hydrogel according to the following formula 2: 溶胀 ):

[0095] W 溶胀 =(W W -W d ) / W d ×100%, in formula 2, W w W0 and W1 are the weight of the hydrogel when it reaches equilibrium and when it is completely dry (g), respectively. The test results are shown in Table 1.

[0096] The porosity of the antibacterial silk nanofiber composite hydrogel obtained in Examples 1 to 4 and Comparative Example 1 was detected by the following method. The porosity test method includes: freezing the obtained antibacterial silk nanofiber composite hydrogel sample at -18°C for 12 hours, then freeze-drying it for 48 hours to obtain a completely dried sample, and then immersing it in anhydrous ethanol with a volume of V1. After immersion for 10 minutes, it is placed in a vacuum oven and evacuated until no visible bubbles escape, and the total volume of the sample immersed in ethanol at this time is recorded as V2. Then take out the sample and record the remaining ethanol volume as V3. Perform 3 parallel experiments, take the average value, and calculate the porosity of the hydrogel according to the following formula 3:

[0097] Porosity (%) = (V1-V3) / (V2-V3)×100%, formula 3. The test results are shown in Table 1.

[0098] The compressive strength of the antibacterial silk nanofiber composite hydrogel obtained in Examples 1 to 4 and Comparative Example 1 was tested according to standard ASTM F2512-20a, and the test was performed 5 times in parallel to obtain the average value. The test results are shown in Table 1.

[0099] Antibacterial test: Test group: The antibacterial silk nanofiber composite hydrogel prepared in Examples 1 to 4 was added to different culture dishes and inoculated with Staphylococcus aureus at a final concentration of 2×10 6 CFU / mL. Control group: The antibacterial silk nanofiber composite hydrogel prepared in Comparative Example 1 was added to a culture dish and inoculated with Staphylococcus aureus at a final concentration of 2×10 6 CFU / mL. Blank group: The culture dish contained only culture medium and was inoculated with Staphylococcus aureus at a final concentration of 2×10 6 CFU / mL. Three parallel samples were made for each group of experiments. The culture dish was placed in a 37℃ incubator for 16 hours. A small amount of bacterial solution (100μL) was added to the surface of the culture medium and evenly spread on the surface of the culture medium with a spreader. The plate was inverted and incubated in a 37℃ incubator for 18 hours. The colonies were counted and the antibacterial rate was calculated. The test results are shown in Table 1.

[0100] Table 1 Test results of antibacterial silk nanofiber composite hydrogel obtained in Examples 1 to 4 and Comparative Example 1

[0101]

[0102] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. An antibacterial silk nanofiber composite hydrogel, It is characterized in that The method comprises the following components: poly-lysine grafted silk nanofibers, a hydrogel matrix and water; The mass ratio of the polylysine grafted silk nanofibers to the hydrogel matrix is ​​1:2-49; The mass content of water in the antibacterial silk nanofiber composite hydrogel is 45-95%; The polylysine grafted silk nanofibers are a supporting skeleton; the polylysine grafted silk nanofibers present a three-dimensional network structure; The hydrogel matrix is ​​a porous structure; the hydrogel matrix is ​​wrapped on the polylysine grafted silk nanofibers and filled in the pores of the polylysine grafted silk nanofibers; The polylysine grafted silk nanofiber is ε-polylysine grafted silk nanofiber.

2. The antibacterial silk nanofiber composite hydrogel according to claim 1, It is characterized in that The content of ε-polylysine in the polylysine grafted silk nanofiber is 0-20wt%, and the content is not zero.

3. The antibacterial silk nanofiber composite hydrogel according to claim 1, It is characterized in that The hydrogel matrix includes one or more of chitosan, chondroitin sulfate, sodium alginate, hyaluronic acid, collagen and gelatin.

4. The antibacterial silk nanofiber composite hydrogel according to claim 1, It is characterized in that The porosity of the antibacterial silk nanofiber composite hydrogel is 50-90%, the equilibrium water absorption rate is 500-1000%, the equilibrium swelling rate is 350-1500%, the compression strength is 0.25-0.5MPa, and the antibacterial rate is greater than 90%.

5. The method for preparing the antibacterial silk nanofiber composite hydrogel according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The poly-lysine grafted silk nanofibers, the hydrogel matrix and water are mixed to obtain a hydrogel precursor; A cross-linking agent is added to the hydrogel precursor to carry out a cross-linking reaction to obtain the antibacterial silk nanofiber composite hydrogel.

6. The preparation method according to claim 5, It is characterized in that The concentration of the hydrogel precursor is 2-10 wt %.

7. The preparation method according to claim 5, It is characterized in that The cross-linking agent includes one or more of glutaraldehyde, glyoxal, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system, genipin, hydrogen peroxide and horseradish peroxidase system, laccase, tyrosinase, methanol, ethanol and calcium chloride; The mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to N-hydroxysuccinimide in the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system is 1:0.2-1; The mass of the cross-linking agent is 0.1-30% of the mass of the hydrogel precursor.

8. The preparation method according to claim 1, It is characterized in that The cross-linking reaction is carried out at a temperature of -25 to 60°C and for a time of 1 to 48 hours.

9. Use of the antibacterial silk nanofiber composite hydrogel according to any one of claims 1 to 4 or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method according to claims 5 to 8 in the preparation of wound dressings.

10. The use according to claim 9, It is characterized in that The wound dressing is one of an antibacterial silk nanofiber composite hydrogel dressing and an antibacterial silk nanofiber composite hydrogel modified textile-based dressing; The antibacterial silk nanofiber composite hydrogel dressing is made of the antibacterial silk nanofiber composite hydrogel according to any one of claims 1 to 4 or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method according to claims 5 to 8; The antibacterial silk nanofiber composite hydrogel modified textile-based dressing comprises a hydrogel functional layer and a textile structure substrate layer; the hydrogel functional layer is loaded on the textile structure substrate layer; the thickness of the hydrogel functional layer is 0.5 to 5 mm; the textile structure substrate layer comprises one of medical absorbent cotton gauze, elastic bandage gauze, wound gauze, non-woven gauze and composite non-woven gauze; The hydrogel in the hydrogel functional layer is the antibacterial silk nanofiber composite hydrogel according to any one of claims 1 to 4 or the antibacterial silk nanofiber composite hydrogel prepared by the preparation method according to claims 5 to 8.

Citation Information

Cited By

  • Preparation method and application of environment-friendly silk fibroin-based antibacterial hydrogel