Diamond synthesis method for optimizing crystal face boron distribution

By using graphite, diboron sulfide and FeNiCo alloy under high temperature and high pressure conditions, and adding Ti/Cu+Al composite nitrogen removal agent, the problem of uneven boron distribution in boron doped diamond is solved, and the uniform distribution of boron in diamond is achieved and high-quality synthesis improves the conductive efficiency and application value of diamond.

CN119056337AInactive Publication Date: 2024-12-03TONGREN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411461097.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, it is difficult to evenly distribute the boron element in boron-doped diamond in the diamond by high-energy particle irradiation method, and the boron distribution is extremely uneven under the high-temperature and high-pressure method, which affects the conductivity efficiency and device performance of the diamond.

Method used

Graphite is used as the carbon source, diboron trisulfide is used as the boron source, FeNiCo alloy is used as the catalyst, and Ti/Cu+Al composite nitrogen removal agent is added under high temperature and high pressure conditions, and the synthesis pressure is controlled to be 5-7GPa and the temperature is 1280-1300. ℃ to optimize the distribution of boron.

Benefits of technology

The uniform distribution of boron in diamond is achieved, the quality and conductivity of diamond are improved, the problem of uneven distribution of boron under high temperature and high pressure conditions is avoided, and the application value of diamond is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056337A_ABST
    Figure CN119056337A_ABST
Patent Text Reader

Abstract

The invention provides a diamond synthesis method for optimizing crystal face boron distribution, which comprises the following steps: graphite is used as a carbon source, diboron trisulfide is used as a boron source, FeNiCo alloy is used as a catalyst, a Ti / Cu + Al composite nitrogen removal agent is added for synthesis, the synthesis pressure is 5-7 GPa, and the synthesis temperature is 1280-1500 DEG C. According to the diamond synthesis method, the nitrogen removal effect is good, the synthesized diamond has very high quality, and the boron concentration distribution of the crystal face of the synthesized diamond (100) is remarkably optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of diamond preparation, and in particular to a diamond synthesis method for optimizing crystal plane boron distribution. Background Art

[0002] Diamond is an extremely functional material that integrates many excellent properties. It has important uses in many fields such as extreme optics, quantum communications, artificial intelligence, heat dissipation materials for high-power laser weapons and chips, ultra-high pressure diamond anvil cells (DAC), substrates for chemical vapor deposition (CVD) large single crystal growth, aerospace, Raman lasers, biomedicine, ultra-fine processing, etc.

[0003] Normally, diamond is an insulator. However, when boron impurities are introduced into diamond, the boron atoms will occupy the carbon atom positions in the lattice in the form of substitution and generate boron acceptors, thereby giving diamond p-type semiconductor properties. The entry of boron atoms into diamond can not only significantly improve the electrical transport properties of diamond semiconductors, but also improve the thermal stability and antioxidant capacity of diamond itself. Boron in diamond can be obtained by irradiating synthesized diamond with high-energy boron particles, and the distribution of boron in the obtained boron-doped diamond is relatively uniform. However, in boron-doped diamonds prepared by this method, boron is often distributed in the surface layer of the diamond, making it difficult to enter its interior. What is particularly important is that diamonds irradiated with high-energy particles will largely destroy the surface structure of the diamond, and produce sp 2 The hybrid graphite phase structure greatly limits its application value.

[0004] High temperature and high pressure method can effectively dope boron into diamond. However, the most critical problem is that the distribution of boron in diamond is extremely uneven. The boron-rich part is blue-black in color. This unevenness is particularly evident in (100) crystal orientation diamond synthesized under high temperature and high pressure conditions. Figure 1 As shown, the unevenness in diamond will directly affect the conductive efficiency of diamond, and will also affect the performance of the device in diamond electronic devices.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for synthesizing diamond, the operating conditions of the method for synthesizing diamond are mild, the whole method is simple to operate, and by adding a composite denitrifier during the synthesis process, the composite denitrifier can reduce the impurity concentration near the diamond growth interface during the synthesis process, which is beneficial to the high temperature and high pressure synthesis of high-quality diamond.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] The invention provides a diamond synthesis method for optimizing crystal plane boron distribution, comprising the following steps: using graphite as a carbon source, diboron trisulfide as a boron source, and FeNiCo alloy as a catalyst, and adding a Ti / Cu+Al composite denitrifier for synthesis, the synthesis pressure is 5-7GPa, and the synthesis temperature is 1280-1300°C.

[0009] In the prior art, the boron-doped diamond obtained by high-energy boron ion irradiation of the prepared diamond only stays on the surface layer of the diamond and is difficult to enter the interior of the diamond. In addition, high-energy particles will destroy the surface structure of the diamond, causing its surface to graphitize.

[0010] In addition, in boron-doped diamond synthesized by high temperature and high pressure method, the distribution of boron inside the diamond is extremely uneven, especially in boron-doped diamond synthesized with (100) crystal plane. In order to completely solve the above problem, the present invention proposes a diamond synthesis method that can solve the above problem.

[0011] The present invention improves the denitrification effect by adding a composite denitrifier on the one hand, and strictly controls the operating conditions on the other hand.

[0012] Of course, the prior art also uses denitrifiers, but the traditional denitrifiers are generally single denitrifiers. However, TiC is inevitably generated during the denitrification process, which will reduce the denitrification effect of Ti to a certain extent. For this reason, the present invention uses this composite denitrifier. The presence of Cu can promote the decomposition of TiC to generate Ti, thereby ensuring the denitrification effect of Ti as much as possible. The introduced Al can directly combine with the impurity nitrogen to generate AlN. Moreover, the density of AlN (3.25g / cm 3 ) is denser than TiC (5.44 g / cm 3 ) is small, and it is easier to float in the molten catalyst, thereby reducing the impurity concentration near the diamond growth interface, which is beneficial to the high temperature and high pressure synthesis of high-quality diamond. Therefore, based on the above principle, the composite denitrification agent used in the present invention is more conducive to the preparation of high-quality diamond.

[0013] Preferably, as a further feasible solution, in the composite denitrifier, the mass ratio of Ti / Cu to Al is (1-10):1.

[0014] Preferably, as a further feasible solution, in the composite denitrifier, the mass ratio of Ti / Cu to Al is (2-6):1.

[0015] Preferably, as a further implementable solution, the mass ratio of Ti / Cu to Al is 5:1.

[0016] As for the ratio of the two, Al mainly plays the role of assisting Ti / Cu to achieve the effect of nitrogen removal, so its addition amount should not be too large. Moreover, if the amount of Al added is too large, due to the low viscosity coefficient of Al, if the amount of Al added is too large, it will have a greater impact on the convection field in the synthesis cavity, which is not conducive to the synthesis of high-quality diamonds. Therefore, its addition amount cannot be too large either.

[0017] Preferably, as a further feasible solution, the addition amount of the composite denitrifier is 0.8-1.5wt% of the catalyst.

[0018] Preferably, as a further feasible solution, the addition amount of the composite denitrifier is 1wt% of the catalyst, because if the addition amount of the denitrifier is too small, the ideal denitrification effect cannot be achieved. If the addition ratio of the denitrifier is too large, it is equivalent to adding excessive impurities in the synthesis system, which is also not conducive to the growth of high-quality diamonds. Therefore, the addition amount should not be too large or too small, and needs to be controlled within an appropriate range.

[0019] Preferably, as a further feasible solution, the synthesis pressure is 6.5 GPa and the synthesis temperature is 1290°C.

[0020] The specific synthesis conditions, especially the synthesis temperature, also need to be strictly controlled, because when the synthesis temperature is high, the (111) crystal plane corresponding to the diamond is very developed, and the (100) crystal plane is very small or even disappears. When the synthesis temperature is low, the (100) crystal plane corresponding to the diamond is very developed, and the (111) crystal plane is very small or even disappears. For this reason, if it is expected to synthesize diamonds with developed (100) crystal planes, the synthesis temperature must be appropriately lowered. If the synthesis temperature is lowered too low, the diamond growth temperature condition will not be reached. Because during the diamond growth process, compared with the (100) crystal plane, boron is more likely to enter the diamond structure along the (111) crystal plane. For this reason, under the premise of reaching the diamond growth temperature condition, the synthesis temperature is lowered as much as possible to ensure that the diamond (100) crystal plane is large enough and the (111) crystal plane is small enough, so as to ensure the uniformity of boron distribution in the (100) crystal plane of the diamond grown in the (100) crystal direction to the greatest extent. Therefore, this temperature needs to be operated according to the temperature range of the present invention.

[0021] The diamond synthesized by the diamond synthesis method of the present invention has higher quality.

[0022] The key structures of diamond synthesis cavity are as follows: Figure 4As shown (longitudinal section), the graphite tube is a heating element, and the temperature in the middle of the graphite tube is the highest. The temperature gradually decreases from the middle position to the upper and lower ends. From the figure, it can be seen that the graphite carbon source is in the high temperature zone, the diamond seed is in the low temperature zone, and the catalyst alloy is between the graphite carbon source and the seed. Since there is a temperature difference between the graphite carbon source and the seed and there is a certain height difference between the two, the temperature difference divided by the height difference is the temperature gradient, which is the driving force for diamond growth. In order to create a good growth environment for diamond growth in the early stage, the denitrification agent is sandwiched between the graphite carbon source and the catalyst alloy. Boron trisulfide powder, which is a boron source, is mixed in the graphite powder and pressed into shape for use.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The diamond synthesis method of the present invention has mild operating conditions, the entire method is simple to operate, and the prepared diamonds have high quality.

[0025] (2) The diamond synthesized by the diamond synthesis method provided by the present invention achieves the effect of optimizing the boron distribution on the crystal surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] By reading the detailed description of the preferred embodiment below, various other advantages and benefits will become clear to those of ordinary skill in the art. The accompanying drawings are only used for the purpose of illustrating the preferred embodiment and are not considered to be limitations of the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings.

[0027] Figure 1 This is a photo of boron-doped diamond with (100) crystal orientation synthesized in the system without nitrogen removal of the present invention;

[0028] Figure 2 A photo of boron-doped diamond with (100) crystal orientation provided in Example 1 of the present invention;

[0029] Figure 3 The time-of-flight secondary ion mass spectrometry test results of the present invention;

[0030] Figure 4 This is a diagram of the key structure of the diamond synthesis cavity. DETAILED DESCRIPTION

[0031] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0032] Example 1

[0033] Synthetic diamond with a particle size of 0.8 mm was used as the seed crystal, and the (100) surface of the seed crystal was selected as the growth interface. Flake FexNiyCoz alloy was selected as the catalyst, each catalyst was 0.5 mm thick and 12 mm in diameter, and a total of 8 pieces were used. High-purity graphite powder with a purity of 99.99% was used as the carbon source for diamond growth, and B was used as the boron source. 2 S 3 (purity of 99.8%) powder is evenly mixed into the graphite carbon source, which accounts for 0.45% of the mass percentage of the carbon source, and the graphite and B 2 S 3 The powder mixture is pre-pressed under a pressure of 5Mpa and then used (with a diameter of 12mm). Ti / Cu and Al are used as composite denitrifiers (1wt% of the catalyst mass). When the mass of Ti / Cu is 0.25g and the mass of Al is 0.05g, the Ti / Cu and Al used are both thin sheets with a thickness of 0.02mm. When assembling the experimental synthesis block, the pre-pressed graphite and boron source are placed at the high-temperature end of the graphite tube, the seed crystal is placed at the low-temperature end of the graphite tube, and the catalyst is placed between the two. The composite denitrifier Ti / Cu+Al flakes are interspersed between the carbon source and the catalyst. The synthesis pressure used in the experiment is 6.5GPa, and the synthesis temperature is 1290℃. The specific results are as follows Figure 1 shown.

[0034] The distribution uniformity of boron in the diamond synthesized by this embodiment is greatly optimized, and the synthesis temperature of the two is the same. Figure 1 and 2 The diamond boron element in the diamond was tested by time-of-flight secondary ion mass spectrometry. The test area is the position marked by the red circle. The test results are as follows Figure 3 shown. Figure 3 (a) is the test result corresponding to the synthesis of boron-doped diamond in the system without nitrogen removal. We can see that there is more boron in the lower half of the figure, while the upper half is black, indicating that this area contains almost no boron. Figure 3 (b) is the boron-doped diamond synthesized by adding diboron trisulfide to the nitrogen removal system in Example 1. It can be observed from this figure that the boron is distributed relatively evenly in the test area.

[0035] Example 2

[0036] The other operation steps are consistent with those in Example 1, except that in the added composite denitrifier, the mass of Ti / Cu is 0.25 g, and the mass of Al is 0.05 g. The specific detection results are consistent with those in Example 1.

[0037] Example 3

[0038] The other operation steps are consistent with those in Example 1, except that in the added composite denitrifier, the mass of Ti / Cu is 0.5 g, and the mass of Al is 0.05 g. The specific detection results are consistent with those in Example 1.

[0039] Example 4

[0040] The other operation steps are consistent with those in Example 1, except that in the added composite denitrifier, the mass of Ti / Cu is 0.05 g, and the mass of Al is 0.05 g. The specific detection results are consistent with those in Example 1.

[0041] Example 5

[0042] The other operation steps are consistent with those in Example 1, except that in the added composite denitrifier, the mass of Ti / Cu is 0.1 g, and the mass of Al is 0.05 g. The specific detection results are consistent with those in Example 1.

[0043] Example 6

[0044] The other operation steps are consistent with those in Example 1, except that in the added composite denitrifier, the mass of Ti / Cu is 0.3 g, and the mass of Al is 0.05 g. The specific detection results are consistent with those in Example 1.

[0045] Example 7

[0046] The other operation steps are consistent with those in Example 1, except that the mass of the composite denitrifier is 0.8wt% of the mass of the catalyst. The mass of the catalyst is calculated based on the mass of the composite denitrifier. The specific test results are consistent with those in Example 1.

[0047] Example 8

[0048] The other operation steps are consistent with those in Example 1, except that the mass of the composite denitrifier is 1.5wt% of the mass of the catalyst. The mass of the catalyst is calculated based on the mass of the composite denitrifier. The specific test results are consistent with those in Example 1.

[0049] Example 9

[0050] The other operation steps are consistent with those in Example 1, except that the synthesis temperature is 1300° C. and the synthesis pressure is 7 GPa. The specific test results are consistent with those in Example 1.

[0051] Example 10

[0052] The other operation steps are consistent with those in Example 1, except that the synthesis temperature is 1280° C. and the synthesis pressure is 5 GPa. The specific test results are consistent with those in Example 1.

[0053] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A diamond synthesis method for optimizing the boron distribution on the crystal surface, It is characterized in that The method comprises the following steps: using graphite as a carbon source, diboron trisulfide as a boron source, and FeNiCo alloy as a catalyst, and adding a composite denitrifier of Ti / Cu+Al for synthesis, with a synthesis pressure of 5-7GPa and a synthesis temperature of 1280-1300°C.

2. The diamond synthesis method according to claim 1, It is characterized in that In the composite denitrifier, the mass ratio of Ti / Cu to Al is (1-10):

1.

3. The diamond synthesis method according to claim 1, It is characterized in that In the composite denitrifier, the mass ratio of Ti / Cu to Al is (2-6):

1.

4. The diamond synthesis method according to claim 1, It is characterized in that The mass ratio of Ti / Cu to Al is 5:

1.

5. The diamond synthesis method according to claim 1, It is characterized in that The addition amount of the composite denitrifier is 0.8-1.5wt% of the catalyst.

6. The diamond synthesis method according to claim 1, It is characterized in that The addition amount of the composite denitrifier is 1wt% of the catalyst.

7. The diamond synthesis method according to claim 1, It is characterized in that The synthesis pressure is 6.5 GPa and the synthesis temperature is 1290°C.

8. Diamond synthesized by the diamond synthesis method according to any one of claims 1 to 7.

Citation Information

Cited By

  • Synthetic method for inhibiting crystal cracking phenomenon of artificial gem-grade diamond