Device and method for producing modified petroleum resin
Through electron beam irradiation technology, the graft modification of mPentadene resin and polarized monomers is solved, and the problem of initiators removing the safety hazards of complex and free radical polymerization reactions in the prior art is achieved, and high efficiency and low cost are achieved The production of modified petroleum resin without the production of "three wastes", achieving green, economical and efficient production.
Patent Information
- Application Number
- CN202411140703.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has complex process of removing initiators or catalysts in the synthesis of modified mPentadene resins, which may reduce product quality, and there are safety hazards and uncontrollable reactions in the free radical polymerization reaction.
Using electron beam irradiation technology, the high-energy electron beam excitation resin generates free radicals, and the graft modification of the interpentadiene resin and polarized monomer is achieved, which avoids the use of initiators or catalysts, simplifies the process flow, and A polar graft monomer recycling tank is set up for recycling.
It improves product quality and reaction efficiency, reduces by-product generation, achieves continuous production, saves 30% of costs, and does not generate "three wastes", achieving green, economical and efficient production.
Smart Images

Figure CN119056364A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to a manufacturing device and a manufacturing method for a modified petroleum resin. Background Art
[0002] Isopentadiene is an important chemical raw material. Its polymer, isopentadiene resin, has good heat resistance, weather resistance and electrical insulation, and is widely used in the fields of electronics, electrical, aerospace, etc. However, since isopentadiene petroleum resin is a non-polar hydrocarbon polymer, its composite force with polar materials is weak, which limits its application field and composite material performance. Therefore, improving its performance through modification technology is one of the current research hotspots. Introducing polar groups into the molecular chain can increase its adhesion and adhesion, improve the softening temperature and compatibility with polar resins, and expand the application range of petroleum resins. In addition, the addition of antioxidants can further improve the stability of the resin and extend its service life.
[0003] In the patent application with the publication number CN104341555A, a method for synthesizing a modified isoprene resin is disclosed. Isoprene, C5 monoolefin, and terpene are used as copolymerization raw materials to prepare a petroleum resin with a smaller molecular weight, a higher softening point, and a lower bromine value. The method for synthesizing the modified isoprene resin includes feeding isoprene, C5 monoolefin, and terpene in a weight ratio of 1: (0.1-0.7): (0.4-1.4) to prepare a copolymerization raw material; under the action of a catalyst, using an inert aliphatic hydrocarbon as a solvent, a cationic polymerization reaction is carried out at a temperature of 30-70°C and an oxygen-free environment to synthesize the resin.
[0004] In the patent application with the publication number CN115572353A, a modified petroleum resin and its preparation method and application are disclosed, wherein the preparation method comprises the following steps: (1) mixing an initiator with heat-insulated isoprene, carrying out a polymerization reaction, and obtaining a petroleum resin solution; (2) mixing the petroleum resin solution after the polymerization reaction in step (1) with an initiator and a polar grafting monomer, carrying out a grafting reaction, and obtaining a modified petroleum resin. The method of the present invention is online and continuous from synthesis to modification, without any intermediate links (traditional: first produce petroleum resin, cut into pellets and package, and then heat and melt for grafting), with low production energy consumption, energy saving, low cost, adjustable grafting rate of modified petroleum resin, and high purity.
[0005] Since isoprene resin contains more unsaturated double bonds, it is convenient to introduce some polar groups. At present, the existing technology mainly focuses on free radical polymerization or cationic polymerization. By adding initiators or catalysts, polar monomers are reacted and polymerized with isoprene resin or isoprene monomers, which increases the process of removing initiators or catalysts. At the same time, incomplete removal of initiators or catalysts will also reduce the quality of modified petroleum resins. Free radical polymerization reactions also have factors such as violent reactions and uncontrollable factors, which pose certain safety hazards. Summary of the invention
[0006] The present application utilizes electron beam irradiation technology and the effect of high-energy electron beams to achieve graft modification of petroleum resins such as piperyl resins with polar monomers. The reaction conditions are mild and there are no potential safety hazards. At the same time, the process is simple, the yield is high, and the product quality is good. In addition, the polar grafted monomers recovered are continuously reused in the reaction.
[0007] Some embodiments of the present application provide a manufacturing device for a modified petroleum resin, comprising: a raw material tank; a devolatilizer, connected to the raw material tank, wherein the outlet of the raw material tank is connected to the inlet of the devolatilizer; a recovery tank, connected to the devolatilizer, wherein the first outlet of the devolatilizer is connected to the inlet of the recovery tank; and a condenser, connected to the recovery tank, wherein the outlet of the recovery tank is bidirectionally connected to the inlet of the condenser, wherein an electron beam irradiation device is provided between the raw material tank and the devolatilizer.
[0008] In some embodiments, there is a pipeline between the raw material tank and the devolatilizer, and the electron beam irradiation device is arranged at the pipeline, wherein the pipeline extends from the raw material tank through the electron beam irradiation device and continuously extends to the devolatilizer, wherein the electron beam irradiation device is nested on the pipeline.
[0009] In some embodiments, the manufacturing device further includes: a feeding pump, which is disposed between the raw material tank and the pipeline and is connected to the pipeline.
[0010] In some embodiments, the manufacturing device also includes: a finished product tank connected to the devolatilizer, wherein the second outlet of the devolatilizer is connected to the inlet of the finished product tank, wherein the second outlet of the devolatilizer is different from the first outlet of the devolatilizer; and a tail gas absorption tank connected to the recovery tank, wherein the first outlet of the recovery tank is connected to the inlet of the tail gas absorption tank, and the second outlet of the recovery tank is connected to the inlet of the raw material tank, wherein the first outlet of the recovery tank is different from the second outlet of the recovery tank.
[0011] Some other embodiments of the present application provide a method for manufacturing a modified petroleum resin, comprising: adding petroleum resin into a raw material tank; adding polarized grafted monomers and antioxidants into the raw material tank, melting and mixing to obtain a mixture; passing the mixture into a devolatilizer through a pipeline via a feeding pump, wherein an electron beam irradiation device is provided between the raw material tank and the devolatilizer, and the mixture enters the devolatilizer after being irradiated with electron beams in the pipeline; and recovering unreacted polarized grafted monomers and oligomers into a recovery tank after condensing them in a condenser through vacuum distillation.
[0012] In some embodiments, the petroleum resin is a molten piperyl resin and the temperature is between 180° C. and 200° C., and wherein the polarized grafting monomer comprises one or more unsaturated olefin functionalized monomers such as maleic anhydride and itaconic anhydride.
[0013] In some embodiments, the mass of the polarized grafting monomer is 1%-10% of the mass of the petroleum resin, and the mass of the antioxidant is 0.1%-1% of the mass of the petroleum resin.
[0014] In some embodiments, the electron beam irradiation device has an electron beam irradiation dose of 100-1000 kGy, an electron energy of the electron beam irradiation is 0.6-1 MeV, and an irradiation time of 10-30 s.
[0015] In some embodiments, adding petroleum resin into the raw material tank includes adding the petroleum resin into the raw material tank under the protection of an inert gas, wherein the inert gas exists in the devolatilizer, and the inert gas in the devolatilizer enters the tail gas adsorption tank for adsorption.
[0016] In some embodiments, after the vacuum distillation, the modified petroleum resin is sent to a granulation workshop for granulation to obtain a modified resin product, wherein the pressure of the vacuum distillation is (-0.07)-(-0.098) MPa, the temperature of the vacuum distillation is 210-220°C, and the time of the vacuum distillation is 30-60 min.
[0017] Compared with the existing technology, the beneficial effects of this application are as follows:
[0018] 1) The present invention can effectively improve the reaction efficiency and product quality by precisely controlling the ratio of maleic anhydride and antioxidant, the dose of electron beam irradiation, the reaction time, and the temperature and time of vacuum distillation. The grafting rate of maleic anhydride in the piperyl-modified petroleum resin produced by the present invention can reach 0.5-7%;
[0019] 2) The present application utilizes electron beam irradiation technology, does not use initiators, reduces the generation of by-products, and is provided with a polar monomer recovery tank to collect the components obtained by devolatilization for subsequent recycling. Compared with the prior art, it can save about 30% of the cost.
[0020] 3) The process is simple, the reaction time is short, and continuous production from feeding to discharging can be achieved. In addition, no "three wastes" are generated in the production process, truly achieving green, economical and efficient production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Aspects of the present invention are best understood from the following detailed description when read with the accompanying figures.
[0022] Figure 1 A flow chart showing a method for producing a modified petroleum resin of the present application. DETAILED DESCRIPTION
[0023] The following disclosure provides many different embodiments or examples for realizing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various embodiments. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0024] Furthermore, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should be interpreted accordingly.
[0025] The present application utilizes electron beam irradiation technology and the effect of high-energy electron beams to realize the grafting modification of petroleum resins such as isoprene resins and polar monomers. Specifically, the present application uses electron beam irradiation technology for grafting, and utilizes the effect of high-energy electron beams to excite the resin to produce free radicals, thereby initiating the grafting reaction. Compared with the prior art, the present technology does not add additional initiators or catalysts, eliminates the process of removing initiators or catalysts, and also avoids the byproducts that may be generated by the initiator-induced free radical reaction; the scheme does not need to add organic solvents to dissolve the resin or polar monomers, eliminating the process of desolventizing; no additional energy is consumed during the reaction, and a polar grafted monomer recovery tank is also provided, which can recycle the unreacted monomers and save costs; the electron beam irradiation technology has the advantage of short reaction time, and the reaction is usually completed within a few seconds or even tens of seconds, which greatly improves the production capacity. The present technology does not produce "three wastes" during the reaction process, and is a green, economical and efficient production process.
[0026] See also Figure 1 , Figure 1 The manufacturing device and related manufacturing process of the modified petroleum resin of the present application are shown. Figure 1 , the manufacturing device of the modified petroleum resin includes: a raw material tank; a devolatilizer, which is connected to the raw material tank, wherein the outlet of the raw material tank is connected to the inlet of the devolatilizer; a recovery tank, which is connected to the devolatilizer, wherein the first outlet of the devolatilizer is connected to the inlet of the recovery tank; and a condenser, which is connected to the recovery tank, wherein the outlet of the recovery tank is bidirectionally connected to the inlet of the condenser. The specific manufacturing process is as follows: the present application adds a certain mass of petroleum resin such as molten isoprene resin into a raw material tank with a stirring device under the protection of an inert gas (such as nitrogen, etc.), and the temperature of the petroleum resin is 180-200°C, in order to make the resin have a better flow state and be able to flow normally in the pipeline; add the polarized grafted monomer and antioxidant in a calculated ratio into the raw material tank for melting and sufficient mixing to obtain a mixture; wherein the rotation speed is 200-300rpm / min; the polarized grafted monomer The monomers include one or more unsaturated olefin functional monomers such as maleic anhydride and itaconic anhydride; the antioxidant includes one of 2,6-di-tert-butyl-4-methylphenol (antioxidant 264) or 3,5-di-tert-butylphenyl-4-hydroxyphenylpropionic acid isooctyl ester (antioxidant 1135); the mass of the polarized grafted monomer is 1%-10% of the mass of the petroleum resin, and the mass of the antioxidant is 0.1%-1% of the mass of the petroleum resin; the mixed material in the raw material tank enters the rear end devolatilization reactor through the feed pump through the pipeline; the flow rate of the pump is 4-12m 3 / h; insulation materials are installed on the pipeline to make the temperature of the pipeline consistent with the temperature in the raw material tank; there is an electron beam irradiation device between the raw material tank and the devolatilizer, and the mixed material enters the pipeline through the feed pump, and enters the devolatilizer after being irradiated by the high-energy electron beam. The electron beam irradiation dose is 100-1000kGy, the electron energy of the electron beam irradiation is 0.6-1MeV, and the irradiation time is 10-30s; after the reaction is completed, the unreacted polarized grafted monomers and oligomers are condensed by the condenser and recovered to the recovery tank through vacuum distillation, wherein the pressure is (-0.07)-(-0.098)Mpa, the vacuum distillation temperature is 210-220℃, and the vacuum distillation time is 30-60min; the recovered polarized grafted monomers are continuously reused in the reaction, and the inert gas (such as nitrogen) in the devolatilizer enters the tail gas adsorption tank for adsorption. After the vacuum distillation is completed, the modified resin is sent to the granulation workshop for granulation to obtain the modified resin product. The process is simple and efficient, and the continuous production of resin is realized. The acid value of the modified petroleum resin can be adjusted, the polarized grafted monomer can be recycled, and no "three wastes" are generated, which truly achieves green and economical production.
[0027] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods for the various indicators of the modified petroleum resin prepared in the following examples are as follows: softening point: ring and ball method (GB / T4507); chromaticity: GB / T22295 (Gardner chromaticity); acid value: GB / T2895, melt viscosity: GB / T24148.4.
[0028] Example 1
[0029] 100 kg of molten isoprene resin was added to a raw material tank with a stirring device under the protection of nitrogen. The temperature of isoprene resin was 180°C. 1 kg of maleic anhydride and 0.1 kg of antioxidant 264 were added to the dosing tank for melting and thorough mixing. The feed pump was turned on and the flow rate was set to 4 m / s. 3 / h; the electron beam irradiation device is 0.6MeV, the electron beam irradiation dose is set to 100KGy, and the reaction time is 30s; the grafted resin enters the rear end devolatilization kettle, and under the conditions of pressure -0.07Mpa and temperature 210°C, the unreacted polarized grafted monomers and oligomers are vacuum distilled to a recovery tank by vacuum distillation, and the vacuum distillation time is 30min; after the vacuum distillation work is completed, the modified isopentylene resin is granulated to obtain a modified isopentylene resin product.
[0030] Example 2
[0031] 100 kg of molten isoprene resin was added to a devolatilizer with a stirring device under the protection of nitrogen, and the temperature of the isoprene resin was 200°C; 5 kg of maleic anhydride and 0.5 kg of antioxidant 264 were added to the dosing tank for melting and thorough mixing; the feed pump was turned on and the flow rate was set to 4 m / s. 3 / h; the electron beam irradiation device is 0.6MeV, the electron beam irradiation dose is set to 100KGy, and the reaction time is 30s; the grafted resin enters the rear end devolatilization kettle, and under the conditions of pressure -0.07Mpa and temperature 210°C, the unreacted polarized grafted monomers and oligomers are vacuum distilled to a recovery tank by vacuum distillation, and the vacuum distillation time is 40min; after the vacuum distillation work is completed, the modified isopentadiene resin is sent to the granulation workshop for granulation to obtain the modified isopentadiene resin product.
[0032] Example 3
[0033] 100 kg of molten isoprene resin was added to a devolatilizer with a stirring device under the protection of nitrogen, and the temperature of the isoprene resin was 200°C; 5 kg of maleic anhydride and 0.5 kg of antioxidant 264 were added to the dosing tank for melting and mixing to obtain a mixed sample; the feed pump was turned on and the flow rate was set to 8 m / s. 3 / h; the electron beam irradiation device is 0.6MeV, the electron beam irradiation dose is set to 500KGy, and the reaction time is 20s; the grafted resin enters the rear end devolatilization kettle, and under the conditions of pressure -0.098Mpa and 220°C, the unreacted polarized grafted monomers and oligomers are vacuum distilled to a recovery tank by vacuum distillation, and the vacuum distillation time is 40min; after the vacuum distillation work is completed, the modified isopentadiene resin is sent to the granulation workshop for granulation to obtain the modified isopentadiene resin product.
[0034] Example 4
[0035] 100 kg of molten isoprene resin is added to a devolatilizer with a stirring device under the protection of inert gas or nitrogen, and the temperature of the isoprene resin is 200°C; 5 kg of maleic anhydride and 0.5 kg of antioxidant 1135 are added to the dosing tank for melting and fully mixing to obtain a mixed sample; the feed pump is turned on and the flow rate is set to 12 m / s. 3 / h; the electron beam irradiation device is 1MeV, the electron beam irradiation dose is set to 1000KGy, and the reaction time is 10s; the grafted resin enters the rear end devolatilization kettle, and the unreacted polarized grafted monomer and oligomer are vacuum distilled to the recovery tank under the conditions of pressure -0.07Mpa and temperature 220℃, and the vacuum distillation time is 60min; the recovered polarized grafted monomer is continuously reused in the reaction. After the vacuum distillation work is completed, the modified isoprene resin is sent to the granulation workshop for granulation to obtain the modified isoprene resin product.
[0036] Example 5
[0037] 100 kg of molten isoprene resin is added to a devolatilizer with a stirring device under the protection of inert gas or nitrogen, and the temperature of the isoprene resin is 200°C; 10 kg of maleic anhydride and 1 kg of antioxidant 264 are added to the dosing tank for melting and fully mixing to obtain a mixed sample; the feed pump is turned on and the flow rate is set to 4 m / s. 3 / h; the electron beam irradiation device is 1MeV, the electron beam irradiation dose is set to 1000KGy, and the reaction time is 30s; the grafted resin enters the rear end devolatilization kettle, and under the conditions of pressure -0.098Mpa and temperature 220°C, the unreacted polarized grafted monomers and oligomers are vacuum distilled to a recovery tank by vacuum distillation, and the vacuum distillation time is 30min; after the vacuum distillation work is completed, the modified isopentadiene resin is sent to the granulation workshop for granulation to obtain the modified isopentadiene resin product.
[0038] Example 6
[0039] 100 kg of molten isoprene resin is added to a devolatilizer with a stirring device under the protection of inert gas or nitrogen. The temperature of isoprene resin is 200°C. 3 kg of maleic anhydride and 0.5 kg of antioxidant 264 and 2 kg of maleic anhydride in the recovery tank are added to the dosing tank for melting and sufficient stirring. The feed pump is turned on and the flow rate is set to 8 m / s. 3 / h; the electron beam irradiation device is 0.6MeV, the electron beam irradiation dose is set to 500KGy, and the reaction time is 20s; the grafted resin enters the rear end devolatilization kettle, and the unreacted polarized grafted monomers and oligomers are vacuum distilled to the recovery tank under the conditions of pressure -0.098Mpa and temperature 220℃, and the vacuum distillation time is 40min; the recovered polarized grafted monomers are continuously reused in the reaction. After the vacuum distillation work is completed, the modified isoprene resin is sent to the granulation workshop for granulation to obtain the modified isoprene resin product.
[0040] Example 7
[0041] 100 kg of molten isoprene resin is added to a devolatilizer with a stirring device under the protection of inert gas or nitrogen. The temperature of isoprene resin is 190°C. 3 kg of itaconic anhydride and 0.5 kg of antioxidant 1135 and 2 kg of itaconic anhydride in the recovery tank are added to the dosing tank for melting and sufficient stirring. The feed pump is turned on and the flow rate is set to 8 m / s. 3 / h; the electron beam irradiation device is 0.8MeV, the electron beam irradiation dose is set to 800KGy, and the reaction time is 20s; the grafted resin enters the rear end devolatilization kettle, and the unreacted polarized grafted monomers and oligomers are vacuum distilled to the recovery tank under the conditions of pressure -0.08Mpa and temperature 220℃, and the vacuum distillation time is 40min; the recovered polarized grafted monomers are continuously reused in the reaction. After the vacuum distillation work is completed, the modified isoprene resin is sent to the granulation workshop for granulation to obtain the modified isoprene resin product.
[0042] The test results of the modified piperylic resin in Examples 1 to 7 are shown in Table 1 below.
[0043] Table 1 Test results of modified piperylene resins of Examples 1 to 7
[0044]
[0045]
[0046] As can be seen from the above table, the present application can effectively improve the reaction efficiency and product quality by precisely controlling the ratio of maleic anhydride and antioxidant, the dose of electron beam irradiation, the reaction time, and the temperature and time of reduced pressure distillation. Specifically, the chromaticity of the modified isoprene resin provided by the method of the present application can be improved to 5 to 8, the acid value can be improved to 3.5 to 39.31 mg KOHg, the softening point can be between 101 and 111° C., and the melt viscosity can be between 150.5 and 283.5 mPa·s.
[0047] Compared with the existing technology, the beneficial effects of this application are as follows:
[0048] 1) The present invention can effectively improve the reaction efficiency and product quality by precisely controlling the ratio of maleic anhydride to antioxidant, the dose of electron beam irradiation, the reaction time, and the temperature and time of vacuum distillation. The grafting rate of maleic anhydride in the isoprene-modified petroleum resin produced by the present invention can reach 0.5-7%.
[0049] 2) The present application utilizes electron beam irradiation technology, does not use initiators, reduces the generation of by-products, and is provided with a polar monomer recovery tank to collect the components obtained by devolatilization for subsequent recycling. Compared with the prior art, it can save about 30% of the cost.
[0050] 3) The process is simple, the reaction time is short, and continuous production from feeding to discharging can be achieved. In addition, no "three wastes" are generated in the production process, truly achieving green, economical and efficient production.
[0051] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that this equivalent construction does not deviate from the spirit and scope of the present invention, and that they can make multiple changes, substitutions and changes herein without departing from the spirit and scope of the present invention.
Claims
1. A manufacturing device for modified petroleum resin, characterized in that: include: Raw material tank; A devolatilizer, connected to the raw material tank, wherein the outlet of the raw material tank is connected to the inlet of the devolatilizer; a recovery tank, connected to the devolatilizer, wherein a first outlet of the devolatilizer is connected to an inlet of the recovery tank; and A condenser is connected to the recovery tank, wherein the outlet of the recovery tank is connected to the inlet of the condenser in a two-way manner. Wherein, an electron beam irradiation device is arranged between the raw material tank and the devolatilization reactor.
2. The manufacturing device according to claim 1, characterized in that: There is a pipeline between the raw material tank and the devolatilizer, and the electron beam irradiation device is arranged at the pipeline. The pipeline extends from the raw material tank through the electron beam irradiation device and continuously extends to the devolatilizer, wherein the electron beam irradiation device is nested on the pipeline.
3. The manufacturing device according to claim 2, characterized in that: Also includes: A feeding pump is arranged between the raw material tank and the pipeline and is connected with the pipeline.
4. The manufacturing device according to claim 1, characterized in that: Also includes: a finished product tank connected to the devolatilizer, wherein a second outlet of the devolatilizer is connected to an inlet of the finished product tank, wherein the second outlet of the devolatilizer is different from the first outlet of the devolatilizer; and A tail gas absorption tank is connected to the recovery tank, wherein a first outlet of the recovery tank is connected to an inlet of the tail gas absorption tank, and a second outlet of the recovery tank is connected to an inlet of the raw material tank, wherein the first outlet of the recovery tank is different from the second outlet of the recovery tank.
5. A method for producing a modified petroleum resin, characterized in that: include: Add petroleum resin into the raw material tank; Adding the polarized grafting monomer and the antioxidant into the raw material tank, melting and mixing, and obtaining a mixed material; The mixed material is fed into a devolatilizer through a feed pump through a pipeline, wherein an electron beam irradiation device is provided between the raw material tank and the devolatilizer, and the mixed material enters the devolatilizer after being irradiated by the electron beam in the pipeline; as well as The unreacted polarized grafted monomers and oligomers are condensed in a condenser by vacuum distillation and then recovered into a recovery tank.
6. The manufacturing method according to claim 5, characterized in that: The petroleum resin is a molten isopyryl resin and the temperature is between 180° C. and 200° C., and the polarized grafting monomer includes one or more unsaturated olefin functionalized monomers such as maleic anhydride and itaconic anhydride.
7. The manufacturing method according to claim 5, characterized in that: The mass of the polarized grafting monomer is 1%-10% of the mass of the petroleum resin, and the mass of the antioxidant is 0.1%-1% of the mass of the petroleum resin.
8. The manufacturing method according to claim 5, characterized in that: The electron beam irradiation device has an electron beam irradiation dose of 100-1000 kGy, an electron energy of 0.6-1 MeV, and an irradiation time of 10-30 s.
9. The manufacturing method according to claim 5, characterized in that: Adding the petroleum resin into the raw material tank includes adding the petroleum resin into the raw material tank under the protection of an inert gas, The inert gas exists in the devolatilizer, and the inert gas in the devolatilizer enters the tail gas adsorption tank for adsorption.
10. The manufacturing method according to claim 5, characterized in that: After the vacuum distillation, the modified petroleum resin is sent to a granulation workshop for granulation to obtain a modified resin product. The pressure of the vacuum distillation is -0.07 to -0.098 MPa, the temperature of the vacuum distillation is 210-220° C., and the time of the vacuum distillation is 30-60 min.
Citation Information
Patent Citations
Synthesis method for modified m-pentadiene resin
CN104341555A
Modified petroleum resin as well as preparation method and application thereof
CN115572353A