Lanthanum-calcium modified attapulgite adsorbent as well as preparation method and application thereof
Through the preparation of lanthanum-calcium modified concave and convex rod soil adsorbent, the problems of high cost of phosphorus pollutants and complex operation in the prior art are solved, and efficient removal of phosphorus pollutants is achieved, meeting sewage discharge standards and reducing treatment costs are achieved. .
Patent Information
- Application Number
- CN202411227738.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
AI Technical Summary
The existing phosphorus pollutant treatment methods have high cost, high requirements on water quality and surrounding environment, and complex operations, especially when dealing with actual sewage, the lack of efficient solid adsorbents.
The preparation method of lanthanum-calcium modified concave and convex rod soil adsorbent is adopted. By mixing concave and convex rod soil, lanthanum salt, calcium salt and sodium hydroxide solution for oscillation reaction, the lanthanum calcium modified concave and convex rod soil composite material is formed to enhance its adsorption. Capability for treating phosphate contaminants in water.
A modified concave and convex rod soil adsorbent with high adsorption capacity has been achieved, which significantly improves the adsorption effect of phosphorus pollutants. After treatment, the concentration of phosphorus pollutants in the sewage can be less than 0.05mg/L, which meets the sewage discharge standards, and the adsorbent can Reused multiple times reduces processing costs.
Smart Images

Figure CN119056397A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adsorption materials, and in particular to a lanthanum-calcium modified attapulgite adsorbent and a preparation method and application thereof. Background Art
[0002] At present, eutrophication of water bodies has become an environmental problem that cannot be ignored in the world. About 40% to 50% of rivers, lakes, reservoirs and other water bodies in the world have experienced varying degrees of eutrophication, and phosphorus is one of the most important factors leading to eutrophication.
[0003] Phosphorus pollution in wastewater is a common environmental problem, severely impacting aquatic ecosystems and human health. Phosphorus is a crucial plant nutrient, but excessive levels can lead to eutrophication, promoting algal growth and ultimately causing algal blooms. Furthermore, phosphorus forms sediments in water, affecting water depth and current velocity, further impacting the habitat of aquatic life.
[0004] Currently, commonly used methods for phosphorus removal from wastewater include biological methods, chemical precipitation, and adsorption, but each has certain drawbacks. Biological methods utilize microorganisms to absorb phosphorus from water. Based on their principles, they can be categorized into two adsorption modes: one in which microorganisms absorb phosphorus from water to meet their own growth and reproduction needs; the other in which specialized microorganisms, called phosphate-accumulating organisms (PAOs), absorb and convert phosphate from wastewater into polyphosphate within their cells under anaerobic or aerobic conditions, where it is then released. This method has been applied to numerous wastewater treatment processes, including SBR, A2 / O, and oxidation ditch processes. Li Wei et al. used an A2 / O-SBR combined process to remove phosphorus from wastewater, achieving a stable total phosphorus removal rate of 95%. They also identified the dominant phosphorus-removing bacteria, DPAO, in this process using high-throughput sequencing and 16S rRNA molecular biotechnology. Biological methods offer numerous advantages for treating phosphorus-containing wastewater, including minimal environmental impact, low energy consumption, simple operation, ease of long-term implementation and maintenance, and low cost. However, biological treatment of phosphorus-containing wastewater takes a long time, and the microorganisms have high requirements for the surrounding environment. In order to maintain suitable living conditions for microorganisms, environmental conditions such as temperature, pH, and organic matter concentration in the water body need to be frequently controlled. In addition, this method will produce a large amount of sludge waste.
[0005] Chemical precipitation involves adding chemical reagents to the wastewater during treatment. These react with phosphates in the wastewater to form a precipitate, which is then removed through filtration and other procedures (Li Qingqing et al., 2022). The basic principle of chemical precipitation is that the smaller the solubility product (Ksp) between the added chemical reagent and the phosphate, the easier it is to form a precipitate, resulting in better phosphorus removal. Currently, commonly used chemical agents for phosphorus removal include aluminum salts, iron salts, and calcium salts. Phosphorus removal by precipitation is influenced by multiple factors, including the actual pH value of the wastewater, various complex substances in the wastewater, phosphorus concentration in the wastewater, and the amount of reagent added (Meng Shunlong et al., 2012). Compared with biological methods, chemical precipitation offers advantages such as simple operation, stable results, and shorter reaction times. However, chemical precipitation has the disadvantages of high cost, high water quality requirements, and high environmental requirements. Furthermore, the addition of large amounts of metal salts to wastewater can easily cause secondary pollution and harm the environment.
[0006] The adsorption method has the advantages of low cost, simple operation, fast reaction and high treatment efficiency, and is therefore widely used in sewage treatment. The so-called adsorption is to use solid particles as adsorbents to fully contact the phosphate in the solution. The phosphate will quickly combine with the active sites on the adsorbent, thereby removing phosphorus from the water solution. The adsorbent as a solid particle can be reused many times after elution, and the concentrated phosphate solution eluted can be simply prepared into phosphate fertilizer for use in farmland. Therefore, the adsorption method can not only effectively alleviate the eutrophication of water bodies, but also effectively recycle phosphate to further utilize phosphorus as a resource. How to disclose a solid adsorbent that can be used to treat phosphorus pollutants in actual sewage is an urgent problem to be solved by those skilled in the art. Summary of the Invention
[0007] The purpose of the present invention is to provide a lanthanum-calcium modified attapulgite adsorbent and its preparation method and application, so as to solve the problems of high cost, high requirements on water quality and surrounding environment, and complex operation in existing phosphorus pollutant treatment methods.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] The invention provides a preparation method of a lanthanum-calcium modified attapulgite adsorbent, comprising the following steps: mixing attapulgite, lanthanum salt, calcium salt, water and sodium hydroxide solution to obtain a mixed material, and performing a shaking reaction to obtain a lanthanum-calcium modified attapulgite composite material.
[0010] Preferably, the usage ratio of the attapulgite, lanthanum salt, calcium salt and water is 2g:0.004-0.016mol:0.004-0.016mol:80-120mL.
[0011] Preferably, the lanthanum salt is lanthanum chloride.
[0012] Preferably, the calcium salt is calcium chloride.
[0013] Preferably, the sodium hydroxide solution is used to adjust the pH value of the reaction system, and the pH value of the mixed material is 10-12.
[0014] Preferably, the concentration of the sodium hydroxide solution is 0.01 to 1 mol / L.
[0015] Preferably, the temperature of the shaking reaction is 25° C., the shaking rate of the shaking reaction is 100 to 300 r / min, and the shaking reaction time is 2 to 5 h.
[0016] The present invention also provides a lanthanum-calcium modified attapulgite adsorbent prepared by the above preparation method.
[0017] The present invention also provides a use of the lanthanum-calcium modified attapulgite adsorbent in treating phosphate pollutants in water.
[0018] The present invention has at least the following beneficial effects:
[0019] The present invention uses La and Ca bimetallic ions to modify attapulgite. La and Ca will produce complementary effects on adsorption sites and adsorption energy barriers, enhancing the adsorption effect of a single metal. A modified attapulgite adsorbent with a high adsorption capacity is prepared, which shows an excellent phosphorus pollutant adsorption effect in treating actual sewage containing multiple pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The graph shows the change in phosphorus content in wastewater as the amount of lanthanum-calcium modified attapulgite adsorbent added is used to treat wastewater containing phosphorus pollutants using the lanthanum-calcium modified attapulgite adsorbent prepared in Example 1. DETAILED DESCRIPTION
[0021] The invention provides a preparation method of a lanthanum-calcium modified attapulgite adsorbent, comprising the following steps: mixing attapulgite, lanthanum salt, calcium salt, water and sodium hydroxide solution to obtain a mixed material, and performing a shaking reaction to obtain a lanthanum-calcium modified attapulgite composite material.
[0022] In the present invention, the usage ratio of the attapulgite, lanthanum salt, calcium salt and water is 2g:0.004~0.016mol:0.004~0.016mol:80~120mL, preferably 2g:0.004~0.016mol:0.004~0.016mol:90~110mL, further preferably 2g:0.004~0.016mol:0.004~0.016mol:95~105mL, more preferably 2g:0.004~0.016mol:0.004~0.016mol:100mL.
[0023] In the present invention, the lanthanum salt is lanthanum chloride, preferably one or more of anhydrous lanthanum chloride, lanthanum chloride heptahydrate and lanthanum chloride pentahydrate.
[0024] In the present invention, the calcium salt is calcium chloride, preferably one or more of anhydrous calcium chloride, dihydrated calcium chloride, tetrahydrated calcium chloride and hexahydrated calcium chloride.
[0025] In the present invention, the sodium hydroxide solution is used to adjust the pH value of the reaction system. The pH value of the mixed material is 10 to 12, preferably 10.5 to 11.5, and more preferably 11.
[0026] In the present invention, the concentration of the sodium hydroxide solution is 0.01 to 1 mol / L, preferably 0.1 to 0.8 mol / L, more preferably 0.3 to 0.6 mol / L, and even more preferably 0.5 mol / L.
[0027] In the present invention, the temperature of the shaking reaction is 0-50°C, preferably 10-40°C, more preferably 20-30°C, and more preferably 25°C; the shaking rate of the shaking reaction is 100-300 r / min, preferably 150-250 r / min, more preferably 180-220 r / min, and more preferably 200 r / min; the shaking reaction time is 2-5 h, preferably 2.5-4.5 h, more preferably 3-4 h, and more preferably 3.5 h.
[0028] In the present invention, after the shock reaction is completed, the steps of separating, washing and drying the lanthanum-calcium modified attapulgite composite material are further included, wherein the separation is centrifugal separation, and the washing is water washing 2 to 5 times; the drying temperature is 90 to 110°C, preferably 95 to 108°C, and more preferably 100 to 105°C, and the drying time is 1.5 to 3 hours, preferably 2 to 2.5 hours.
[0029] The present invention also provides a lanthanum-calcium modified attapulgite adsorbent prepared by the above preparation method.
[0030] The present invention also provides a use of the lanthanum-calcium modified attapulgite adsorbent in treating phosphate pollutants in water.
[0031] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0032] Example 1
[0033] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 3.7 g of LaCl₃·7H₂O and 1.11 g of CaCl₂ (La:Ca molar ratio of 1:1) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 81.15 mg / g for phosphorus.
[0034] Example 2
[0035] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 2.46 g of LaCl₃·7H₂O and 1.46 g of CaCl₂ (La:Ca molar ratio of 1:2) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 79.32 mg / g for phosphorus.
[0036] Example 3
[0037] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 1.85 g of LaCl₃·7H₂O and 1.65 g of CaCl₂ (a molar ratio of La to Ca of 1:3) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 78.36 mg / g for phosphorus.
[0038] Example 4
[0039] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 1.48 g of LaCl₃·7H₂O and 1.77 g of CaCl₂ (La:Ca molar ratio of 1:4) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 59.26 mg / g for phosphorus.
[0040] Example 5
[0041] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 4.93 g of LaCl₃·7H₂O and 0.74 g of CaCl₂ (a molar ratio of La to Ca of 2:1) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After completion of the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 79.14 mg / g for phosphorus.
[0042] Example 6
[0043] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 5.55 g of LaCl₃·7H₂O and 0.55 g of CaCl₂ (La:Ca molar ratio of 3:1) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 81.14 mg / g for phosphorus.
[0044] Example 7
[0045] 2 g of 200-mesh attapulgite was mixed with 100 mL of deionized water and stirred for 30 minutes to achieve uniform mixing. 5.92 g of LaCl₃·7H₂O and 0.44 g of CaCl₂ (La:Ca molar ratio of 4:1) were then added and magnetically stirred for 1 hour to achieve uniform mixing. The pH of the system was adjusted to 10 with 1 mol / L NaOH solution. The mixture was then shaken at 160 rpm for 2 hours at a constant temperature (25°C). After the reaction, the mixture was centrifuged (9000 rpm for 10 minutes). The precipitate was washed three times with deionized water and then dried in an oven at 105°C for 2 hours to obtain a lanthanum-calcium-modified attapulgite adsorbent with an adsorption capacity of 79.68 mg / g for phosphorus.
[0046] Comparative Example 1
[0047] The adsorption capacity of unmodified attapulgite for phosphorus pollutants is 5.6 mg / g.
[0048] The adsorption performance of the lanthanum-calcium modified attapulgite adsorbent prepared in Example 1 was tested using aquaculture wastewater containing high concentrations of phosphate from Ninghe District, Tianjin. The test results are as follows: Figure 1 As shown, from Figure 1 It can be seen that with the increase in the amount of adsorbent used, the concentration of phosphorus pollutants in the sewage gradually decreases. When the amount of adsorbent added is 2g / L, the concentration of phosphorus pollutants in the treated sewage can be as low as 0.035mg / L, which is lower than the 0.05mg / L in the sewage TP discharge standard.
[0049] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing a lanthanum-calcium modified attapulgite adsorbent, characterized in that: The method comprises the following steps: mixing attapulgite, lanthanum salt, calcium salt, water and sodium hydroxide solution to obtain a mixed material, and performing a shaking reaction to obtain a lanthanum-calcium modified attapulgite composite material.
2. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to claim 1, characterized in that: The dosage ratio of the attapulgite, lanthanum salt, calcium salt and water is 2g: 0.004-0.016mol: 0.004-0.016mol: 80-120mL.
3. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to claim 2, characterized in that: The lanthanum salt is lanthanum chloride.
4. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to any one of claims 1 to 3, characterized in that: The calcium salt is calcium chloride.
5. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to claim 4, characterized in that: The sodium hydroxide solution is used to adjust the pH value of the reaction system, and the pH value of the mixed material is 10-12.
6. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to claim 5, characterized in that: The concentration of the sodium hydroxide solution is 0.01-1 mol / L.
7. The method for preparing a lanthanum-calcium modified attapulgite adsorbent according to claim 6, characterized in that: The temperature of the shaking reaction is 0-50° C., the shaking rate of the shaking reaction is 100-300 r / min, and the shaking reaction time is 2-5 h.
8. The lanthanum-calcium modified attapulgite adsorbent prepared by the preparation method of the lanthanum-calcium modified attapulgite adsorbent according to any one of claims 1 to 7.
9. Use of the lanthanum-calcium modified attapulgite adsorbent according to claim 8 in treating phosphate pollutants in water.
Citation Information
Cited By
Modified attapulgite adsorbent as well as preparation method and application thereof
CN120037887A