Kaolin-based solid amine carbon dioxide adsorbent and preparation method thereof
A kaolin-based carbon dioxide adsorbent is developed by modifying kaolin with NaOH and HCl and loading TEPA, addressing the limitations of existing adsorbents by enhancing adsorption capacity and stability without structural damage, achieving up to 153 mg/g CO2 adsorption.
Patent Information
- Application Number
- CN202411359916.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-27
AI Technical Summary
Existing carbon dioxide adsorbents face issues such as high corrosiveness, volatility, high energy consumption, limited adsorption capacity, and stability, with amine-functionalized solid adsorbents having high costs and complex preparation processes, while porous materials have limited physical adsorption effects.
A kaolin-based solid amine carbon dioxide adsorbent is prepared by modifying kaolin with NaOH and HCl solutions to increase its specific surface area, followed by loading organic amines like tetraethylenepentamine (TEPA) to enhance adsorption performance without damaging the kaolin structure.
The method results in a high-performance carbon dioxide adsorbent with increased specific surface area and improved adsorption capacity, achieving CO2 adsorption capacities of up to 153 mg/g, while retaining the kaolin structure and maintaining stability through multiple cycles.
Smart Images

Figure CN119056399A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon dioxide adsorbents, and in particular to a kaolin-based solid amine carbon dioxide adsorbent and a preparation method thereof. Background Art
[0002] The efficient, energy-saving and environmentally friendly capture materials in the existing CO2 capture technology mainly include liquid amines, carbon-based adsorbents, zeolite-based adsorbents, metal organic framework (MOFs)-based adsorbents, porous polymer-based adsorbents and amine-functionalized solid adsorbents. At present, liquid amines are highly corrosive to equipment, volatile, and have high renewable energy consumption; porous materials have only physical adsorption effects, so their adsorption capacity and adsorption rate are limited, and the adsorption stability needs to be further improved; amine-functionalized solid adsorbents have attracted much attention due to their low cost, physical-chemical synergistic adsorption, low energy requirements and good stability.
[0003] For example: Chinese patent application number 202211720326.2 discloses a carbon-based solid amine carbon dioxide adsorbent and a preparation method thereof. The carbon-based solid amine carbon dioxide adsorbent is prepared by grafting a carbon-based carrier with a grafting modifier, and then impregnating and dispersing the carbon-based carrier with an impregnation modifier and a surfactant. Using mesoporous carbon or carbon nanotubes as a carrier, ultrasound-assisted grafting modification is first performed, and then impregnation modification is performed and a surfactant is added for dispersion. The prepared adsorbent material has a high amino utilization rate and has good adsorption performance for CO2, while significantly improving the cyclic stability of the adsorbent. However, its carrier cost is high and the preparation process is complicated.
[0004] The Chinese patent with application number 202111645042.7 discloses a method for preparing a gasification slag-based solid amine carbon dioxide adsorbent, which belongs to the technical field of carbon dioxide adsorbents. An organic amine-gasification slag composite adsorbent is prepared by loading one or a mixture of organic amines such as polyethyleneimine, pentaethylenehexamine, and ethanolamine. The preparation method of the composite adsorbent is: dissolve the organic amine in an ethanol solution, add the gasification ash residue carbon material, stir and impregnate it thoroughly, evaporate the solvent in a 75°C water bath, and dry it overnight to obtain the amine-loaded gasification ash residue carbon composite adsorbent. However, the CO2 adsorption performance of the amine-loaded gasification ash residue carbon composite adsorbent prepared by it is average. Summary of the invention
[0005] The purpose of the present invention is to provide a kaolin-based solid amine carbon dioxide adsorbent and a preparation method thereof in view of the above-mentioned deficiencies of the prior art. The present invention increases the specific surface area of kaolin to load organic amines while retaining a good kaolin structure to obtain a high-performance carbon fixation material.
[0006] The method for preparing a kaolin-based solid amine carbon dioxide adsorbent of the present invention comprises the following steps:
[0007] S1, sequentially modifying kaolin with NaOH solution and HCl solution to obtain alkali-acid modified kaolin;
[0008] S2, adding alkali-acid modified kaolin to an ethanol solution of tetraethylenepentamine, stirring for reaction, and then drying and grinding to obtain the kaolin-based solid amine carbon dioxide adsorbent.
[0009] Furthermore, the specific process of NaOH solution modification is: adding kaolin to a NaOH solution with a concentration of 15-20%, stirring for reaction in a water bath, centrifuging, washing, drying and grinding to obtain alkali-modified kaolin.
[0010] Furthermore, the mass volume ratio of kaolin to NaOH solution is 5 g:50 mL.
[0011] Furthermore, the specific process of HCl solution modification is: after the alkali-modified kaolin and the HCl solution with a concentration of 1-6M are stirred in a water bath for reaction, the reaction is centrifuged, washed, dried and ground to obtain the alkali-acid modified kaolin.
[0012] Furthermore, the mass volume ratio of the alkali-modified kaolin to the HCl solution is 1-2 g:15 mL.
[0013] Furthermore, the water bath reaction temperature for the NaOH solution modification and the HCl solution modification is 80-85°C.
[0014] Further, the purity of kaolin is 85-99%.
[0015] Furthermore, the mass ratio of the alkali-acid modified kaolin to the organic amine is 1:0.1-0.9.
[0016] Furthermore, in step S2, the stirring speed of the stirring reaction is 100-300 r / min, and the reaction time is 1-12 h.
[0017] A kaolin-based solid amine carbon dioxide adsorbent prepared by the above preparation method.
[0018] The present invention uses kaolin treated with appropriate acid and alkali to increase the specific surface area without destroying the crystal structure, thereby promoting the loading amount of organic amines, and further improving the carbon dioxide adsorption performance to the best. Inappropriate acid and alkali treatment will destroy the structure of kaolin, increase the specific surface area, and load organic amines to improve the carbon dioxide adsorption performance to a certain extent, but it is much worse than the carbon dioxide adsorption performance of kaolin without destroying the crystal structure.
[0019] The kaolin in the kaolin-based solid amine carbon dioxide adsorbent prepared by the present invention still retains the intrinsic structure of kaolin after treatment and has a high specific surface area. The main peak (001) intensity of the treated kaolin is >800 and the bun peak of the amorphous substance is not obvious. Specific surface area>25m 2 The carbon dioxide adsorption capacity of the treated kaolin loaded with 10-90% TEPA is increased to 35-153 mg / g.
[0020] The treated kaolinite of the present invention is loaded with an organic amine (TEPA) by an impregnation method to prepare a carbon dioxide adsorbent. Theoretical calculations show that among the four organic amines, TEPA has the largest interaction energy with kaolinite and the most stable binding. TEPA has the largest adsorption energy with CO2, and the organic amine has the best adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The kaolin with a purity of 85.9% in Example 1 X-ray powder diffraction pattern of
[0022] Figure 2 Prepared in Example 1 X-ray powder diffraction pattern of
[0023] Figure 3 The theoretically calculated interaction energy maps of kaolinite and ethylenediamine (EDA), polyethyleneimine (PEI), diethylenetriamine (DETA) and tetraethylenepentamine (TEPA);
[0024] Figure 4 The theoretically calculated adsorption energy diagram of CO2 adsorption by ethylenediamine (EDA), polyethyleneimine (PEI), diethylenetriamine (DETA) and tetraethylenepentamine (TEPA);
[0025] Figure 5 This is a comparison chart of the carbon dioxide adsorption capacity of the adsorbent prepared in Example 1;
[0026] Figure 6 Prepared in Example 1 Cycle performance;
[0027] Figure 7 Prepared in Example 1 Infrared spectra before and after adsorption of CO2;
[0028] Figure 8 Prepared in Example 1 and Comparison of X-ray photoelectron spectra;
[0029] Fig. 9 Prepared in Example 1 X-ray photoelectron spectrum of N1s;
[0030] Fig.10 The X-ray powder diffraction pattern of kaolin ZT-1 with a purity of 98% in Example 2;
[0031] Fig.11 The X-ray powder diffraction pattern of ZT-1-HCl-NaOH prepared in Example 2;
[0032] Fig.12 This is a comparison chart of the carbon dioxide adsorption capacity of the adsorbent prepared in Example 2;
[0033] Fig.13 The X-ray powder diffraction pattern of ZT-1-HCl-NaOH-TEPA-80% prepared in Example 3;
[0034] Fig.14 Prepared in Comparative Example 1 and X-ray powder diffraction patterns of ZT-1-HCl-NaOH;
[0035] Fig.15 Prepared for this comparative example 1 Comparison of carbon dioxide adsorption capacity of ZT-1-HCl-NaOH. DETAILED DESCRIPTION
[0036] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0037] Embodiment 1:
[0038] Preparation of kaolin-based solid amine material in this example
[0039] Kaolin with a purity of 85.9% Take 5g and add 50mL of 15% NaOH in a water bath at 85℃, stir at 200r / min, and react for 1h. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain
[0040] Take another 2g Add 15 mL of 6M HCl in a water bath at 80°C, stir at 200 r / min, and react for 80 min. After the reaction, centrifuge at 8000 r / min, wash with deionized water until the pH is neutral, dry in an oven at 80°C, cool to room temperature, take out and grind thoroughly to obtain
[0041] Then 1g Add 0.1-0.8g tetraethylenepentamine (TEPA) to 20mL ethanol in which it has been dissolved, stir at 200r / min, and react for 12h. After the reaction, put it in an oven at 80℃ to dry for 12h, cool it to room temperature, take it out and grind it thoroughly to obtain a powdered sample
[0042] The CO2 adsorption performance of the material was measured by a thermogravimetric analyzer. The instrument was a German company, NETZSCH, model STA449C. The protective atmosphere was set to N2 (99.99%), the purge atmosphere was 50mL / min CO2 (99.99%), about 10mg of the sample was taken and placed in an alumina crucible, and heating was started from the greenhouse, and the temperature was raised to 100℃ at a rate of 10℃ / min. The adsorption was maintained for 60min under 50mL / min N2 atmosphere to remove the interference source, and the adsorption atmosphere CO2 was turned on after cooling to the selected temperature, and the adsorption was maintained for 120min, and the adsorption curve was recorded. The CO2 adsorption amount of the material is shown in Formula 1-1:
[0043]
[0044] See attached Figure 1 , which is kaolin with a purity of 85.9% in the technical solution of this embodiment The X-ray powder diffraction pattern of kaolin The main phase is kaolinite, and it also has potassium feldspar mixed peaks (Microcline).
[0045] See attached Figure 2 , prepared according to the technical solution of this embodiment X-ray powder diffraction pattern. The kaolinite crystal structure is not destroyed and the mantou peak of amorphous material is not obvious.
[0046] See Table 1, which is prepared according to the technical solution of this embodiment. The structural characteristics of. The specific surface area is 216.78m 2 / g.
[0047] See attached Figure 3 , is the theoretical calculated interaction energy spectrum of kaolinite with ethylenediamine (EDA), polyethyleneimine (PEI), diethylenetriamine (DETA) and tetraethylenepentamine (TEPA). It shows that TEPA is most likely to interact strongly with the kaolinite crystal surface. This shows that TEPA among the four organic amines is most likely to combine with kaolinite and is easy to load on kaolinite. Therefore, kaolin can be used as an excellent carrier for loading TEPA.
[0048] See attached Figure 4 , is the theoretical calculated adsorption energy diagram of CO2 adsorption by ethylenediamine (EDA), polyethyleneimine (PEI), diethylenetriamine (DETA) and tetraethylenepentamine (TEPA) in the technical solution of this embodiment. According to the order of adsorption energy, TEPA>EDA>DETA>PEI. Therefore, from the perspective of organic amine adsorption of CO2, theoretical calculation shows that TEPA is the best loading substance for adsorbing CO2.
[0049] See attached Figure 5 , prepared according to the technical solution of this embodiment Comparison of carbon dioxide adsorption capacity. As the TEPA loading increases, The CO2 adsorption capacity first increases and then decreases. The increase in loading will lead to The pores are blocked, which is not conducive to CO 2 Diffusion and adsorption. The CO2 adsorption capacity is the largest, which is 134.44 mg / g.
[0050] See attached Figure 6 , prepared according to the technical solution of this embodiment The carbon dioxide cycle performance is good. The cycle experiment was adsorbed at 85℃ and desorbed at 110℃. After 15 cycles, the CO2 adsorption amount remained at 105.18mg / g.
[0051] See attached Figure 7 , prepared according to the technical solution of this embodiment Infrared spectra of before and after the adsorption of CO2. The NH (3374, 3285 and 1570 cm -1 ) and CH(1475cm -1 ) peak is formed This shows that TEPA is indeed loaded on kaolin. After CO2 adsorption, CO (1416cm -1 ) peak appears, which indicates Adsorbed CO2. The reaction equations of primary amine and secondary amine contained in TEPA with CO2 are shown in 1-2 and 1-3.
[0052]
[0053] See attached Figure 8 and Fig. 9 According to the technical solution of this embodiment and After TEPA modification, sharp XPS peaks appeared at the binding energy centers of 285.3 (C 1s), 399.5 eV (N 1s), and 532 eV (O 1s), indicating that There are amine groups in the sample. In order to further analyze the chemical properties of N, Fig. 9 In this paper, we studied the N1s region in high-resolution XPS spectra and pointed out that The N1s binding energies of the different chemically active N species are approximately 398.8 eV, 399.4 eV, and 401.0 eV, respectively. The main N1s peak with a binding energy of 398.9 eV can be attributed to C-NH-C. The two peaks at 399.4 eV and 401.0 eV can be attributed to -NH2 and -NH from the amine group, respectively. 3+ This corresponds to the primary and secondary amines of TEPA.
[0054] The present invention provides a CO2 solid adsorbent containing TEPA loaded on low-purity kaolin after acid-base treatment The main peak (001) intensity of the treated low-purity kaolin is >800 and the bun peak of the amorphous substance is not obvious. After the specific surface area is increased and 60% TEPA is loaded, the CO2 adsorption capacity reaches a maximum of 134.44 mg / g.
[0055] Embodiment 2:
[0056] This example prepares kaolin-based solid amine material ZT-1-HCl-NaOH-TEPA-30-80%.
[0057] Take 5g of kaolin ZT-1 with a purity of 98%, add 50mL of 15% NaOH in a water bath at 85℃, stir at 200r / min, and react for 1h. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain ZT-1-NaOH.
[0058] Take 2g of ZT-1-NaOH, add 15mL of 6M HCl in a water bath at 80℃, stir at 200r / min, and react for 80min. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain ZT-1-HCl-NaOH.
[0059] Then, 1g of ZT-1-HCl-NaOH was added with 0.3-0.8g of tetraethylenepentamine (TEPA) into 20mL of ethanol in which it had been dissolved, stirred at 200r / min, and reacted for 12h. After the reaction, it was placed in an oven at 80℃ for 12h, cooled to room temperature, taken out and fully ground to obtain a powdered sample ZT-1-HCl-NaOH-TEPA-30~80%.
[0060] The CO2 adsorption performance of ZT-1-HCl-NaOH-TEPA-30~80% was measured by thermogravimetric analyzer. The instrument was STA449C from NETZSCH, Germany. The protective atmosphere was set to N2 (99.99%), the purge atmosphere was 50mL / min CO2 (99.99%), about 10mg of sample was taken and placed in an alumina crucible, and heated from the greenhouse, and heated to 100℃ at a rate of 10℃ / min, and adsorbed for 60min under 50mL / min N2 atmosphere to remove interference sources, and then cooled to the selected temperature and the adsorption atmosphere CO2 was turned on, and the adsorption was kept warm for 120min, and the adsorption curve was recorded. The CO2 adsorption amount of the material is shown in Formula 1-1.
[0061] See attached Fig.10 , is the X-ray powder diffraction spectrum of kaolin ZT-1 with a purity of 98% in the technical solution of this embodiment. The result shows that it contains fewer impurity peaks, mainly kaolinite.
[0062] See attached Fig.11 , is the X-ray powder diffraction pattern of ZT-1-HCl-NaOH prepared according to the technical scheme of this embodiment. The kaolinite crystal structure of ZT-1-HCl-NaOH is not destroyed.
[0063] See Table 2 for the structural characteristics of ZT-1-HCl-NaOH prepared according to the technical solution of this embodiment. The specific surface area of ZT-1-HCl-NaOH is 239.61 m 2 / g.
[0064] See attached Fig.12 , which is a comparison chart of the carbon dioxide adsorption of ZT-1-HCl-NaOH-TEPA-30% to ZT-1-HCl-NaOH-TEPA-80% prepared according to the technical scheme of this embodiment. With the increase of TEPA loading, the CO2 adsorption of ZT-1-HCl-NaOH also increases first and then decreases. The CO2 adsorption of ZT-1-HCl-NaOH-70% is the largest, which is 153 mg / g.
[0065] The present invention provides a CO2 solid adsorbent ZT-1-HCl-NaOH-TEPA-30-80% of high-purity kaolin loaded with TEPA after acid-base treatment. The main peak (001) intensity of the treated high-purity kaolin is greater than 800, and its specific surface area increases to 239.61m 2 / g, after loading 70% TEPA, the CO2 adsorption capacity reaches a maximum of 153mg / g. Compared with Example 1, it is proved that under the premise of retaining a good kaolin structure, increasing the specific surface area and loading more organic amine (TEPA) can obtain a high-performance carbon fixation material.
[0066] Embodiment 3:
[0067] This example prepares kaolin-based solid amine material ZT-1-HCl-NaOH-TEPA-80%.
[0068] Take 5g of kaolin ZT-1 with a purity of 98%, add 50mL of 20% NaOH in a water bath at 85℃, stir at 200r / min, and react for 1h. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain ZT-1-NaOH.
[0069] Take 2g of ZT-1-NaOH, add 15mL of 6M HCl in a water bath at 80℃, stir at 200r / min, and react for 80min. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain ZT-1-HCl-NaOH.
[0070] Then, 1g of ZT-1-HCl-NaOH was added to 0.8g of tetraethylenepentamine (TEPA) in 20mL of ethanol in which it had been dissolved, stirred at 200r / min, and reacted for 12h. After the reaction, it was placed in an oven at 80℃ for 12h, cooled to room temperature, taken out and fully ground to obtain a powdered sample ZT-1-HCl-NaOH-TEPA-80%.
[0071] The CO2 adsorption performance of ZT-1-HCl-NaOH-TEPA-80% was measured by a thermogravimetric analyzer. The instrument was selected from the German company NETZSCH, model STA449C. The protective atmosphere was set to N2 (99.99%), the purge atmosphere was 50mL / min CO2 (99.99%), about 10mg of the sample was taken and placed in an alumina crucible, and heating was started from the greenhouse, and the temperature was raised to 100℃ at a rate of 10℃ / min. The adsorption was maintained for 60min under 50mL / min N2 atmosphere to remove the interference source, and the adsorption atmosphere CO2 was turned on after cooling to the selected temperature, and the adsorption was maintained for 120min, and the adsorption curve was recorded. The CO2 adsorption amount of the material is shown in Formula 1-1.
[0072] See attached Fig.13 , is the X-ray powder diffraction pattern of ZT-1-HCl-NaOH prepared according to the technical scheme of this embodiment. The kaolinite crystal structure of ZT-1-HCl-NaOH is not destroyed.
[0073] The present invention provides a CO2 solid adsorbent ZT-1-HCl-NaOH-TEPA-80% of high-purity kaolin loaded with TEPA after acid-base treatment. The main peak (001) intensity of the treated high-purity kaolin is greater than 800, and its specific surface area is increased to 266.49 m 2 / g, after loading 80% TEPA, the CO2 adsorption capacity reached a maximum of 166.67 mg / g. Compared with Example 2, it is proved that under the premise of retaining a good kaolin structure, adjusting the acid-base treatment steps to further increase the specific surface area and load more organic amines (TEPA) can obtain high-performance carbon fixation materials.
[0074] Comparative Example 1:
[0075] This comparative example prepares kaolin-based solid amine material and ZT-1-HCl-NaOH-80%.
[0076] Three different purities of kaolinite ores (Purity: 67.5%) Take 5g of ZT-1 and add 50mL of 25% NaOH in a water bath at 85℃, stir at 200r / min, and react for 1h. After the reaction, centrifuge at 8000r / min, wash with deionized water until the pH is neutral, dry in an oven at 80℃, cool to room temperature, take out and grind thoroughly to obtain and ZT-1-NaOH.
[0077] Take another 2g Add 30 mL of 6M HCl to ZT-1-NaOH in a water bath at 80°C, stir at 200 r / min, and react for 80 min. After the reaction, centrifuge at 8000 r / min, wash with deionized water until the pH is neutral, dry in an oven at 80°C, cool to room temperature, take out and grind thoroughly to obtain and ZT-1-HCl-NaOH.
[0078] Then 1g Add 0.8g tetraethylenepentamine (TEPA) and ZT-1-HCl-NaOH to 20mL ethanol in which they have been dissolved, stir at 200r / min, and react for 12h. After the reaction, put it in an oven at 80℃ for 12h, cool it to room temperature, take it out and grind it thoroughly to obtain a powdered sample. and ZT-1-HCl-NaOH-TEPA-80%.
[0079] The CO2 adsorption performance of ZT-1-HCl-NaOH-TEPA-80% was measured by thermogravimetric analyzer. The instrument was STA449C from NETZSCH, Germany. The protective atmosphere was set to N2 (99.99%), the purge atmosphere was 50mL / min CO2 (99.99%), about 10mg of sample was taken and placed in an alumina crucible, and heated from the greenhouse, and heated to 100℃ at a rate of 10℃ / min, and adsorbed for 60min under 50mL / min N2 atmosphere to remove interference sources, and then cooled to the selected temperature and opened the adsorption atmosphere CO2, and adsorbed for 120min at a temperature of 120min, and the adsorption curve was recorded. The CO2 adsorption amount of the material is shown in Formula 1-1.
[0080] See attached Fig.14 , prepared according to the technical solution of this comparative example and ZT-1-HCl-NaOH X-ray powder diffraction patterns. The kaolin structure after alkali and acid treatment is destroyed, the main peak disappears, the crystallinity deteriorates, and the bun peak of amorphous material appears. The kaolin structure is maintained relatively well.
[0081] See Table 3, which is prepared according to the technical solution of this embodiment. and structural characteristics of ZT-1-HCl-NaOH. The specific surface area is 405.91m 2 / g, The specific surface area is 343.23m 2 / g, the specific surface area of ZT-1-HCl-NaOH is 536.06m 2 / g. The smallest specific surface area.
[0082] See attached Fig.15 , prepared according to the technical solution of this comparative example Comparison of carbon dioxide adsorption between ZT-1-HCl-NaOH and ZT-1-HCl-NaOH. Under the same conditions as ZT-1-HCl-NaOH, 80% TEPA was loaded. The CO2 adsorption capacity was ranked as follows: ZT-1-HCl-NaOH, 122.58mg / g>79.88mg / g>70.67mg / g. Specific surface area is 343.23m 2 / g On the contrary, CO2 has the largest adsorption capacity. This is related to the layered structure of kaolin. XRD results show that the structure is least damaged and the crystal structure is best preserved. Compared with Example 1 and Example 2, it can also be verified that when the kaolin structure is destroyed and a mantou peak exists, the CO2 adsorption capacity of TEPA loaded with a high specific surface area is also lower than that of TEPA loaded with kaolin with a complete structure and a low specific surface area.
[0083] The CO2 solid adsorbent of TEPA loaded on kaolin treated with high concentration acid and alkali provided in Comparative Example 1 and ZT-1-HCl-NaOH-80%. The CO2 adsorption capacity of ZT-1-HCl-NaOH-80% was 79.88mg / g, 122.58mg / g and 70.67mg / g respectively. The acid-base treatment of kaolin with too high concentrations caused its structure to collapse and its specific surface area to increase. Although it can still load TEPA and have a certain CO2 adsorption performance, the CO2 adsorption performance is poor compared with the kaolin loaded with TEPA with a complete structure and a small specific surface area after low concentration treatment.
[0084] Table 1
[0085]
[0086] Table 2
[0087]
[0088] Table 3
[0089]
[0090] For matters not mentioned above, the prior art applies.
[0091] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a kaolin-based solid amine carbon dioxide adsorbent, Features: The following steps are involved: S1, sequentially modifying kaolin with NaOH solution and HCl solution to obtain alkali-acid modified kaolin; S2, adding alkali-acid modified kaolin to an ethanol solution of tetraethylenepentamine, stirring for reaction, and then drying and grinding to obtain the kaolin-based solid amine carbon dioxide adsorbent.
2. The preparation method according to claim 1, Features: The specific process of NaOH solution modification is: adding kaolin to a NaOH solution with a concentration of 15-20%, stirring for water bath reaction, centrifugation, washing, drying and grinding to obtain alkali-modified kaolin.
3. The preparation method according to claim 1, Features: The mass volume ratio of kaolin and NaOH solution is 5g:50mL.
4. The preparation method according to claim 2, Features: The specific process of HCl solution modification is: after the alkali-modified kaolin is reacted with HCl solution with a concentration of 1-6M in a water bath by stirring, the reaction is then centrifuged, washed, dried and ground to obtain the alkali-acid-modified kaolin.
5. The preparation method according to claim 4, Features: The mass volume ratio of alkali-modified kaolin and HCl solution is 1-2 g:15 mL.
6. The preparation method according to claim 4, Features: The water bath reaction temperature for NaOH solution modification and HCl solution modification is 80-85°C.
7. The preparation method according to claim 1, Features: The purity of kaolin is 85-99%.
8. The preparation method according to claim 1, Features: The mass ratio of alkali-acid modified kaolin to organic amine is 1:0.1-0.
9.
9. The preparation method according to claim 1, Features: In step S2, the stirring reaction is carried out at a stirring speed of 100-300 r / min and the reaction is carried out for 1-12 h.
10. A kaolin-based solid amine carbon dioxide adsorbent prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
CO2 adsorbent and preparation method thereof
CN114700043A
Preparation method and application of amine modified CO2 adsorption acid activated attapulgite material
CN116393098A
High-purity kaolin-based carbon dioxide adsorbent and preparation method thereof
CN118681529A