Air separation adsorbent and preparation method thereof

The composite adsorbent structure with a low-silicon X molecular sieve inner layer and high-silicon MFI molecular sieve outer layer addresses the desorption challenges of carbon dioxide and water vapor, enhancing nitrogen and oxygen separation performance by preventing their adsorption and enabling quick desorption, thereby improving oxygen concentration.

CN119056403AActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310623420.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

Existing air separation adsorbents using low-silicon X molecular sieves face challenges in quickly desorbing carbon dioxide and water vapor, leading to reduced nitrogen and oxygen separation performance due to their strong binding ability, which results in decreased efficiency and deactivation.

Method used

A composite adsorbent structure is developed with an inner layer of low-silicon X molecular sieve and an outer layer of high-silicon MFI molecular sieve, where the outer layer prevents water vapor and carbon dioxide from entering the inner layer, and the binder adsorbs these gases during pressure reduction, allowing for quick desorption and improved separation performance.

Benefits of technology

The composite structure enhances nitrogen and oxygen separation performance by preventing water vapor and carbon dioxide from affecting the inner adsorbent layer, resulting in higher oxygen concentration and improved adsorbent efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004256118540000011
    Figure HDA0004256118540000011
  • Figure HDA0004256118540000012
    Figure HDA0004256118540000012
  • Figure HDA0004256118540000021
    Figure HDA0004256118540000021
Patent Text Reader

Abstract

The air separation adsorbent comprises an inner adsorbent layer and an outer adsorbent layer, the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, the outer adsorbent layer comprises an MFI molecular sieve and a binder, the cation site of the low-silicon X molecular sieve is occupied by Li, and the MIF molecular sieve is a high-silicon MFI molecular sieve or an all-silicon MFI molecular sieve. The adsorbent is used for pressure swing adsorption separation of nitrogen and oxygen in air and preparation of oxygen-rich gas, and has good separation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an air separation adsorbent and a preparation method thereof, in particular to an air separation adsorbent with X molecular sieve as an active component and a preparation method thereof. Background Art

[0002] Oxygen can be widely used in many fields such as metallurgy, chemical industry, and environmental protection. By using pressure swing adsorption (PSA) technology to separate nitrogen from other gases in the air, oxygen-rich gas with an oxygen concentration of more than 90% can be obtained. The active component of the pressure swing adsorption separation adsorbent is usually X molecular sieve. The X molecular sieve and clay are mixed evenly in a certain proportion, and the adsorbent balls are obtained after rolling, drying, and roasting.

[0003] CN1146374A discloses an adsorbent for a cyclic pressure swing adsorption process, the adsorbent containing a framework SiO2 / Al2O3 molar ratio of 2.0 to 2.4 and 60 to 89% (equivalent) Ca ++ Cation, 10-40% (equivalent) Na + Cations and 0-10% (equivalent) K + Cationic zeolite X, Ca ++ 、Na + and K + Providing a total cation equivalent of at least 90%, this X-type zeolite is much more effective as an adsorbent for air separation in a pressure swing adsorption process at 50-20°C and 5-506.5 kPa (0.05-5.0 atm) than the same X-type zeolite which has been calcium exchanged to a greater or lesser extent.

[0004] CN101708456A discloses a molecular sieve adsorbent for oxygen production by pressure swing adsorption air separation and a preparation method thereof. The active component of the adsorbent is Ca2O3 with SiO2 / Al2O3=2.0-2.1. 2+ Exchanged low silicon X-type molecular sieve, in which Ca 2+ The exchange degree is 80-100%. Since the exchange of calcium-type X molecular sieve with high exchange degree is difficult and costly, calcium chloride solution is used to exchange low-silicon X molecular sieve to reduce the cost.

[0005] CN1158139C discloses an improved binder zeolite adsorbent, whose active component is a deep lithium exchanged X molecular sieve with a Si / Al atomic ratio of 1. Multiple exchanges with lithium chloride solution can obtain a higher lithium exchange rate and nitrogen adsorption capacity.

[0006] CN1291907A discloses an improved PSA adsorbent whose active component is LiX zeolite material. The intrinsic mass transfer rate of the PSA adsorbent is improved by using an appropriate amount of agglomerated binder that can be converted into zeolite by alkali cooking ("CD") and adding combustible fibers or particulate materials during the molding process to improve the macroporous structure.

[0007] CN104138741A discloses a rare earth modified lithium low silicon molecular sieve adsorbent and a preparation method thereof. The method can significantly improve the hydrothermal stability and help prolong the service life by introducing rare earth elements into the cavity structure of the lithium low silicon molecular sieve.

[0008] During the pressure swing adsorption separation process, carbon dioxide, water vapor, etc. in the air will also be adsorbed by the low-silicon X-ray distillation molecular sieve adsorbent. However, due to the strong binding ability of carbon dioxide and water vapor with the low-silicon X-ray distillation molecular sieve, these gases are difficult to desorb quickly when the system pressure is reduced, resulting in a significant decrease in the separation performance of the adsorbent or even deactivation. Summary of the invention

[0009] The purpose of the present invention is to provide an air separation adsorbent based on the prior art, which is used for pressure swing adsorption separation of nitrogen and oxygen in the air to produce high-concentration oxygen and has high nitrogen and oxygen separation performance.

[0010] The air separation adsorbent provided by the present invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises an MFI molecular sieve and a binder, wherein the cation position of the low-silicon X molecular sieve is occupied by Li, and the MIF molecular sieve is a high-silicon MFI molecular sieve or a full-silicon MFI molecular sieve.

[0011] The present invention also provides a method for preparing an air separation adsorbent, comprising the following steps:

[0012] (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as the inner adsorbent layer, and then a powder of MFI molecular sieve and binder mixed in a mass ratio of 10-60:40-90 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening;

[0013] (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours;

[0014] (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

[0015] The present invention also provides a method for preparing oxygen from air using the nitrogen-oxygen separation adsorbent of the present invention or the nitrogen-oxygen separation adsorbent prepared by the method provided by the present invention.

[0016] The air separation adsorbent provided by the present invention adopts a composite layer structure, wherein the outer adsorbent layer comprises a hydrophobic high-silicon MFI molecular sieve or a full-silicon MFI molecular sieve and a binder. During the adsorption process, the high-silicon MFI molecular sieve or the full-silicon MFI molecular sieve can prevent a small amount of water vapor from entering the outer layer of the adsorbent, and the binder adsorbs carbon dioxide and remaining water vapor in the air, thereby preventing carbon dioxide and water vapor from being adsorbed by the low-silicon X molecular sieve of the inner adsorbent layer, resulting in a decrease in the nitrogen and oxygen separation capacity of the adsorbent; since the binder has a relatively weak adsorption capacity for carbon dioxide and water vapor, the carbon dioxide and water vapor adsorbed by the outer adsorbent layer during the pressure reduction and purging process can be quickly removed, thereby reducing the influence of the carbon dioxide and water vapor on the low-silicon X molecular sieve, and facilitating the improvement of the nitrogen and oxygen separation performance of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of pressure swing adsorption device.

[0018] Figure 2 This is a scanning electron microscope (SEM) photograph of the low silicon X molecular sieve in Example 1.

[0019] Figure 3 This is a scanning electron microscope (SEM) photograph of the all-silicon MFI molecular sieve in Example 1. DETAILED DESCRIPTION

[0020] The nitrogen-oxygen separation adsorbent provided by the present invention is rolled into two batches. First, a mixture of a low-silicon X molecular sieve with a high nitrogen adsorption capacity and a binder is rolled into small balls as an inner adsorbent layer, and then a mixture of a high-silicon MFI molecular sieve or a full-silicon MFI molecular sieve and a binder is added and rolled to form an outer adsorbent layer to prepare a composite layer adsorbent. During pressure swing adsorption, during the process of increasing pressure, the high silicon MFI molecular sieve or all-silicon MFI molecular sieve of the outer adsorbent layer can prevent a small amount of water vapor in the air from entering the outer layer of the adsorbent, and the binder can adsorb carbon dioxide and remaining water vapor in the air to prevent them from entering the inner adsorbent layer. After the remaining air enters the inner adsorbent layer, nitrogen is selectively adsorbed, and the remaining gas passes through the adsorbent bed and is discharged to obtain oxygen-rich gas; during the process of reducing pressure, the nitrogen previously adsorbed by the low silicon X molecular sieve of the inner adsorbent layer is desorbed. At the same time, since the binder of the outer adsorbent layer has a weak adsorption capacity for water and carbon dioxide, the adsorbed carbon dioxide and water vapor can be quickly removed and discharged together with the nitrogen desorbed from the inner adsorbent layer, thereby effectively solving the problem of the nitrogen and oxygen separation performance of the low silicon X molecular sieve being reduced due to the adsorption of carbon dioxide and water vapor, and increasing the concentration of the obtained oxygen, thereby improving the overall nitrogen and oxygen separation performance of the composite layer adsorbent.

[0021] The air separation adsorbent provided by the present invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises an MFI molecular sieve and a binder, wherein the cation position of the low-silicon X molecular sieve is occupied by Li, and the MIF molecular sieve is a high-silicon MFI molecular sieve or a full-silicon MFI molecular sieve.

[0022] The air separation adsorbent provided by the present invention comprises: the inner adsorbent layer comprises 50-79 mass % of low-silicon X molecular sieve and 21-50 mass % of binder, based on the total amount of the inner adsorbent layer; the outer adsorbent layer comprises 10-60 mass % of MFI molecular sieve and 40-90 mass % of binder, and based on the total amount of the outer adsorbent layer, the proportion of the inner adsorbent layer in the adsorbent is 90-96 mass %.

[0023] In the air separation adsorbent provided by the present invention, the silicon oxide / aluminum oxide molar ratio of the low silicon X molecular sieve is 1.90-2.05, the grain size of the low silicon X molecular sieve is 0.4-10 microns, and the Li2O content in the low silicon X molecular sieve is greater than or equal to 10 mass%.

[0024] In the air separation adsorbent provided by the present invention, the silicon oxide / aluminum oxide molar ratio of the high silicon MFI molecular sieve is greater than 200, preferably greater than 500, more preferably greater than 800, and the crystal particle size of the MFI molecular sieve is 0.1 to 0.8 microns.

[0025] In the air separation adsorbent provided by the present invention, the binder is selected from one of kaolin, halloysite and attapulgite.

[0026] The water content of the air separation adsorbent provided by the present invention is less than or equal to 0.6% by mass.

[0027] The air separation adsorbent provided by the present invention is preferably in the form of small spheres, and the average particle size of the small spheres is 300 to 850 microns.

[0028] The preparation method of the air separation adsorbent provided by the present invention comprises the following steps:

[0029] (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as the inner adsorbent layer, and then a powder of MFI molecular sieve and binder mixed in a mass ratio of 10-60:40-90 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening;

[0030] (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours;

[0031] (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

[0032] Wherein, the cation position of the low silicon X molecular sieve described in step (1) is occupied by Li, the cation position of the Y molecular sieve is occupied by at least one of Na or K, the mass of the inner adsorbent layer is 90-96% of the mass of the inner adsorbent layer and the outer adsorbent layer; the low silicon X molecular sieve and the MFI molecular sieve are prepared by conventional methods in the art, which will not be described here. The equipment for rolling ball forming can be a turntable, a sugar coating pan or a drum. When rolling ball forming, the uniformly mixed solid raw materials are placed in a rotating device, and water is sprayed while rolling to make the solid powder adhere and agglomerate into small balls. The amount of water added during rolling ball forming is 5-16% of the total mass of the solid, preferably 8-12%. After rolling into balls, the small balls are sieved to obtain small balls with a particle size of 300-850 microns.

[0033] In the method for preparing an air separation adsorbent provided by the present invention, in step (2), the small balls obtained in step (1) are spread flat to form a bed layer with uniform thickness, and the thickness of the bed layer is preferably less than or equal to 20 mm. During the drying process, air needs to continuously pass through the bed layer to quickly take away the water vapor. In order to prevent high-temperature water vapor from destroying the molecular sieve in the small balls, the air stays in the adsorbent bed layer for less than or equal to 20 seconds, preferably less than or equal to 15 seconds.

[0034] In the preparation method of the air separation adsorbent provided by the present invention, in step (3), the small balls obtained in step (2) are laid flat to form a bed layer with uniform thickness, the thickness of the bed layer is preferably less than or equal to 15 mm, and the calcination is carried out in 4 stages, the calcination temperature is preferably 160-200°C, 270-300°C, 370-400°C, 460-500°C, the constant temperature calcination time of each stage is preferably 2-3 hours, 2-3 hours, 2-3 hours, 5-6 hours, the heating rate is 0.5-5°C / min, preferably 1-3°C / min, during the calcination process, air needs to continuously pass through the bed layer to quickly take away the water vapor, in order to avoid high-temperature water vapor from destroying the molecular sieve in the small balls, the air stays in the adsorbent bed layer for less than or equal to 20 seconds, preferably less than or equal to 15 seconds. After the calcination process is completed, the adsorbent small balls are cooled to room temperature under vacuum conditions.

[0035] The adsorbent provided by the present invention is suitable for separating nitrogen and oxygen in the air by pressure swing adsorption to produce high-concentration oxygen. The pressure swing adsorption can be carried out in a double-column or multi-column manner, or by using a rotary valve or a solenoid valve group to realize the pressure swing adsorption process. The operating pressure is 0.2-0.5MPa, and the operating temperature is 5-50°C.

[0036] A double-column pressure swing adsorption device is used to evaluate the adsorbent performance. The schematic diagram of the pressure swing adsorption device is shown in Figure 1 As shown in the figure, the device consists of a pressure gauge, an adsorption column, a solenoid valve, etc. The four steps of boosting, adsorption, depressurization, and purging are performed by opening or closing the solenoid valves V1, V2, V3, V5, V6, V7, and V8 to achieve continuous generation of oxygen-rich gas. About 370 mL of adsorbent is loaded in adsorption columns A and B respectively, and the adsorption is set to 3s, and the depressurization, purging, and boosting are set to 3s in total. The maximum pressure of the adsorption column is 0.25MPa, the operating temperature is 35°C, and the oxygen-rich gas generation rate is 4.5L / h. After 50 consecutive cycles, the oxygen volume concentration in the product is analyzed using an oxygen concentration meter.

[0037] Method for determining the moisture content of the adsorbent: place an adsorbent with a mass of m1 in a crucible and calcine it at 600°C for 2 hours. After calcination, quickly take out the crucible and place it in a dryer to cool to room temperature. Weigh the mass of the adsorbent after calcination as m2, and the moisture content of the adsorbent C = (m1-m2) / m1.

[0038] The present invention is further described below by way of examples, but the present invention is not limited thereto.

[0039] The following examples are used to prepare the adsorbents described in the present invention.

[0040] The preparation methods of low silicon X molecular sieve, high silicon MFI molecular sieve and full silicon MFI molecular sieve in the examples of the present invention are as follows:

[0041] Low silicon X molecular sieve: 4.66kg sodium hydroxide, 7.23kg potassium hydroxide, 35.74kg deionized water, 47.57kg low alkalinity sodium aluminate solution (Al2O3 mass fraction of 11.0%, Na2O mass fraction of 15.1%) and 36.72kg water glass are added to the reactor, stirred and mixed to form a molecular sieve synthesis system. The total molar ratio of each material in the molecular sieve synthesis system is: SiO2 / Al2O3=2.40, M2O / SiO2=2.25, H2O / SiO2=45, where M is K and Na, K / (K+Na)=0.23. The above molecular sieve synthesis system is transferred to the reactor, aged at 70°C for 6 hours, hydrothermally crystallized at 95°C for 12 hours, filtered, and the obtained solid is washed with deionized water until the filtrate pH is 8-9, and dried at 80°C for 12 hours to obtain a low silicon X molecular sieve.

[0042] A 1.5 mol / L lithium chloride solution was prepared, and the pH was adjusted to 8-10 with lithium hydroxide. The lithium chloride solution and the low silicon X molecular sieve were mixed at a liquid-to-solid ratio of 5 L / kg, and exchanged at 80°C for 1 hour, and repeated 7 times. The exchanged low silicon X molecular sieve was dried at 40°C for 10 hours to obtain a low silicon X molecular sieve with lithium cation.

[0043] The molar ratio and Li2O content of the low silicon X molecular sieve can be adjusted by adjusting the molar ratio of SiO2 / Al2O3 in the molecular sieve synthesis system, the concentration of the lithium chloride solution, and the liquid-solid ratio of the lithium chloride solution to the low silicon X molecular sieve.

[0044] High silicon MFI molecular sieve: 70.77kg tetrapropylammonium hydroxide solution, 6.09kg sodium hydroxide, 130.32kg deionized water, 6.39kg aluminum sulfate solution, 290.41kg silica sol and 4.36kg all-silicon MFI molecular sieve were added into the reactor and stirred to form a molecular sieve synthesis system. The total molar ratio of each material in the molecular sieve synthesis system is: SiO2 / Al2O3=0.0025, OH - / SiO2=0.15,H2O / SiO2=15,R / SiO2=0.06,S / SiO2=0.05,wherein R is tetrapropylammonium hydroxide and S is all-silicon MFI molecular sieve. The molecular sieve synthesis system is transferred to a reaction kettle, hydrothermally crystallized at 150℃ for 48 hours, filtered, and the obtained solid is washed with deionized water until the filtrate pH is 8-9, and dried at 80℃ for 12 hours to obtain a high-silicon MFI molecular sieve.

[0045] All-silicon MFI molecular sieve: 37.91 kg of tetrapropylammonium hydroxide solution and 26.67 kg of silica sol were added into the reactor and stirred to form a molecular sieve synthesis system. The total molar ratio of each material in the molecular sieve synthesis system is: OH - / SiO2=0.35, H2O / SiO2=19.6, R / SiO2=0.35, where R is tetrapropylammonium hydroxide. The molecular sieve synthesis system was transferred to a reactor, aged at 100℃ for 12 hours, hydrothermally crystallized at 150℃ for 48 hours, filtered, and the obtained solid was washed with deionized water until the filtrate pH was 8-9, and dried at 80℃ for 12 hours to obtain a full-silicon MFI molecular sieve.

[0046] Example 1

[0047] (1) Molding: 75 kg of low silicon X molecular sieve with a particle size of about 0.5 μm (SEM photo see Figure 2 , the molar ratio of silicon oxide to aluminum oxide is 2.03, and the content of Li2O is 11.9% by mass) and 25 kg of kaolin are mixed evenly, put into a rotating disk and rolled while spraying water to make the solid aggregate into small balls as the core, and then 0.53 kg of all-silicon MFI molecular sieve with a particle size of about 0.4 μm is added (SEM photo see Figure 3 ) and 4.74 kg of attapulgite powder, continue to spray water and roll to form the outer layer of small balls, and after sieving, small balls with a particle size of 300 to 850 microns are obtained.

[0048] (2) Drying: The beads prepared in step (1) were evenly spread to a bed thickness of 10 mm, and dried at 100°C in a flowing air atmosphere with the air staying in the adsorbent bed for 15 seconds. The drying was performed for 10 hours.

[0049] (3) Calcination: The small balls dried in step (2) were evenly spread out to a bed thickness of 8 mm and calcined in a flowing air atmosphere with the air staying in the adsorbent bed for 8 seconds. The balls were treated at 200°C for 3 hours, 300°C for 3 hours, 400°C for 3 hours, and 500°C for 6 hours at a heating rate of 2°C / min. After calcination, the temperature was cooled to room temperature under vacuum to obtain adsorbent A.

[0050] The water content and separation performance of adsorbent A are shown in Table 1.

[0051] Example 2

[0052] Adsorbent B was prepared according to the method of Example 1, except that in step (1), 2.63 kg of a mixed powder of all-silicon MFI molecular sieve with a particle size of about 0.4 μm and 2.63 kg of attapulgite was added, and water spraying and rolling were continued to form the outer layer of the spheres.

[0053] The water content and separation performance of adsorbent B are shown in Table 1.

[0054] Example 3

[0055] Adsorbent C was prepared according to the method of Example 1, except that 0.95 kg of a mixed powder of all-silicon MFI molecular sieve with a particle size of about 0.4 μm and 6.78 kg of attapulgite was added in step (1), and water spraying and rolling were continued to form the outer layer of the small balls. The water content and separation performance of adsorbent C are shown in Table 1.

[0056] Example 4

[0057] Adsorbent D was prepared according to the method of Example 1, except that a high-silicon MFI molecular sieve with a particle size of about 0.5 μm and a silicon oxide / aluminum oxide molar ratio of 282 was used in step (1).

[0058] The water content and separation performance of adsorbent D are shown in Table 1.

[0059] Example 5

[0060] Adsorbent E was prepared according to the method of Example 4, except that a low-silicon X molecular sieve with a particle size of about 4 μm (silicon oxide / aluminum oxide molar ratio of 1.93 and Li2O content of 10.7 mass %) was used in step (1).

[0061] The water content and separation performance of adsorbent E are shown in Table 1.

[0062] Example 6

[0063] Adsorbent F was prepared according to the method of Example 1, except that the bed thickness in step (2) was 18 mm and the drying temperature was 100° C. The bed thickness in step (3) was 15 mm and the heating rate was 3° C. / min.

[0064] The water content and separation performance of adsorbent F are shown in Table 1.

[0065] Example 7

[0066] Adsorbent G was prepared according to the method of Example 1, except that in step (2), it was dried at 100°C for 8 hours, and in step (3), it was treated at 180°C for 2 hours, 280°C for 2 hours, 380°C for 2 hours, and 470°C for 5 hours.

[0067] The water content and separation performance of adsorbent G are shown in Table 1.

[0068] Comparative Example 1

[0069] Adsorbent H was prepared according to the method of Example 1, except that (1) molding: 75 kg of low-silicon X molecular sieve (silicon oxide / aluminum oxide molar ratio of 2.03, Li2O content of 11.9 mass %) with a particle size of about 0.5 μm and 25 kg of kaolin were mixed evenly, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls, and after screening, small balls with a particle size of 300 to 850 μm were obtained.

[0070] The water content and separation performance of adsorbent H are shown in Table 1.

[0071] Comparative Example 2

[0072] Adsorbent I was prepared according to the method of Example 1, except that the bed thickness in step (2) was 35 mm and the residence time of air in the adsorbent bed was 25 seconds.

[0073] The water content and separation performance of adsorbent I are shown in Table 1.

[0074] Comparative Example 3

[0075] Adsorbent J was prepared according to the method of Example 1, except that the bed thickness in step (3) was 35 mm and the residence time of air in the adsorbent bed was 25 seconds.

[0076] The water content and separation performance of adsorbent J are shown in Table 1.

[0077] Comparative Example 4

[0078] Adsorbent K was prepared according to the method of Example 1, except that the heating rate in step (3) was 10°C / min.

[0079] The water content and separation performance of adsorbent K are shown in Table 1.

[0080] Comparative Example 5

[0081] Adsorbent L was prepared according to the method of Example 1, except that step (3) did not use staged calcination, but directly raised the temperature to 500° C. and calcined for 6 h.

[0082] The water content and separation performance of adsorbent L are shown in Table 1.

[0083] Comparative Example 6

[0084] Adsorbent M was prepared according to the method of Example 1, except that in step (3), the adsorbent was treated at 200°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour, respectively.

[0085] The water content and separation performance of adsorbent M are shown in Table 1.

[0086] Table 1

[0087] Instance number Adsorbent No. Water content, mass% Oxygen volume concentration, % 1 A 0.29 95.2 2 B 0.30 95.0 3 C 0.29 94.3 4 D 0.30 94.8 5 E 0.32 94.5 6 F 0.25 94.0 7 G 0.53 95.0 Comparative Example 1 H 0.33 83.6 Comparative Example 2 I 0.25 76.1 Comparative Example 3 J 0.13 39.6 Comparative Example 4 K 0.23 72.8 Comparative Example 5 L 0.20 63.5 Comparative Example 6 M 3.45 85.2

[0088] It can be seen from Table 1 that the oxygen volume concentration obtained by separating air using the adsorbents described in Comparative Examples 1 to 6 is lower than that of the adsorbents described in Examples 1 to 7.

[0089] The adsorbent described in Comparative Example 1 does not contain an outer adsorbent layer, and carbon dioxide and water vapor in the air are adsorbed by the low-silicon X molecular sieve, resulting in a decrease in its nitrogen and oxygen separation performance.

[0090] In Comparative Example 2, when preparing the adsorbent I, due to the thick bed thickness in step (2), the air stays in the adsorbent bed for a long time, resulting in excessive contact time between water vapor and the adsorbent during the drying process, which destroys the structure of the molecular sieve and reduces the separation performance of the adsorbent. At the same time, since the molecular sieve structure is destroyed, the water absorption capacity of the adsorbent is reduced, so the water content of the adsorbent is low.

[0091] In comparative example 3, when preparing the adsorbent J, the bed thickness in step (3) is relatively thick, and the air stays in the adsorbent bed for a long time, resulting in excessive contact time between water vapor and the adsorbent during the roasting process, which destroys the structure of the molecular sieve, reduces the separation performance of the adsorbent, and reduces the water content.

[0092] In comparative example 4, when preparing the adsorbent K, the heating rate in step (3) was too fast, which resulted in the destruction of the molecular sieve structure, reduced separation performance of the adsorbent, and decreased water content.

[0093] In comparative example 5, when preparing the adsorbent L, step (3) does not use staged calcination, resulting in too fast a heating rate, which leads to the destruction of the molecular sieve structure, the decrease of the separation performance of the adsorbent, and the reduction of the water content.

[0094] In Comparative Example 6, when preparing the adsorbent M, the calcination time was too short and the maximum temperature was too low, resulting in a higher water content in the adsorbent and a decrease in the adsorption and separation performance.

Claims

1. An air separation adsorbent, characterized in that: The invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises an MFI molecular sieve and a binder. The cation position of the low-silicon X molecular sieve is occupied by Li, and the MIF molecular sieve is a high-silicon MFI molecular sieve or a full-silicon MFI molecular sieve.

2. The adsorbent according to claim 1, characterized in that The inner adsorbent layer comprises 50-79 mass % of low-silicon X molecular sieve and 21-50 mass % of binder, based on the total amount of the inner adsorbent layer.

3. The adsorbent according to claim 1, characterized in that The outer adsorbent layer comprises 10-60 mass % of the MFI molecular sieve and 40-90 mass % of the binder, based on the total amount of the outer adsorbent layer.

4. The adsorbent according to claim 1, characterized in that The silicon oxide / aluminum oxide molar ratio of the low silicon X molecular sieve is 1.90-2.05, and the silicon oxide / aluminum oxide molar ratio of the high silicon MFI molecular sieve is greater than 200.

5. The adsorbent according to claim 1, characterized in that The proportion of the inner adsorbent layer in the adsorbent is 90 to 96% by mass.

6. The adsorbent according to claim 1, characterized in that The crystal grain size of the low-silicon X molecular sieve is 0.4 to 10 microns.

7. The adsorbent according to claim 1, characterized in that The content of Li2O in the low-silicon X molecular sieve is greater than or equal to 10 mass %.

8. The adsorbent according to claim 1, characterized in that The silicon oxide / aluminum oxide molar ratio of the high-silicon MFI molecular sieve is greater than 500.

9. The adsorbent according to claim 1, characterized in that The crystal particle size of the MFI molecular sieve is 0.1 to 0.8 microns.

10. The adsorbent according to claim 1, characterized in that The binder is selected from one of kaolin, halloysite and attapulgite.

11. The adsorbent according to claim 1, characterized in that The water content of the adsorbent is less than or equal to 0.6% by mass.

12. A method for preparing the nitrogen-oxygen separation adsorbent according to claim 1, characterized in that: The following steps are involved: (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as the inner adsorbent layer, and then a powder of MFI molecular sieve and binder mixed in a mass ratio of 10-60:40-90 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening; (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours; (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

13. The method according to claim 12, characterized in that In step (1), the total amount of water added for rolling into balls is 5 to 16% by weight of the total amount of solid powder.

14. The method according to claim 12, characterized in that In step (2) or (3), the residence time of air in the adsorbent bed is less than or equal to 20 seconds.

15. The method according to claim 12, characterized in that The staged calcination in step (3) has a heating rate of 0.5 to 5°C / min, preferably 1 to 3°C / min.

16. A method for preparing oxygen from air using the adsorbent according to claims 1 to 11 or the air separation adsorbent prepared by the method of claims 12 to 15.

Citation Information

Patent Citations

  • X / ZSM-5 core / shell molecular sieve and preparation method thereof

    CN108264052A

  • A para-xylene adsorbent and a preparing method thereof

    CN108525643A

  • X / Silicalite-1 core / shell molecular sieve and preparation method thereof

    CN108525650A

  • Improved adsorbent composition

    CN1345628A