Preparation method and application of sodium alginate / nano-zinc oxide composite adsorbent

By using chitosan as a modifier in sodium alginate/nano zinc oxide composite materials, the problem of poor adsorption effect of pure sodium alginate is solved, the adsorption and mechanical properties of the composite materials are improved, and it is suitable for wastewater treatment.

CN119056413APending Publication Date: 2024-12-03HUBEI YUEHUA TESTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310632437.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The adsorption effect of pure sodium alginate as an adsorbent is not ideal, and the sodium alginate/nanozinc oxide composite material has problems such as strong hydrophilicity, poor mechanical properties, and poor dispersion effect of nano zinc oxide.

Method used

Using chitosan as a modifier, using a mixed solution of hydrochloric acid and citric acid to dissolve sodium alginate and nano zinc oxide, and prepare sodium alginate/nano zinc oxide composite materials through dissolution, dispersion and self-assembly to form better adsorption Composite adsorbents with properties.

Benefits of technology

It improves the adsorption performance, mechanical properties and dispersion effect of nano zinc oxide, provides better adsorption performance for wastewater treatment, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056413A_ABST
    Figure CN119056413A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a sodium alginate / nano-zinc oxide composite adsorbent, and the preparation method of the sodium alginate / nano-zinc oxide composite adsorbent comprises the following steps: respectively preparing a hydrochloric acid solution and a citric acid solution, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution; respectively dissolving sodium alginate, nano-zinc oxide and chitosan by using the mixed solution as a solvent to prepare a sodium alginate solution, a nano-zinc oxide solution and a chitosan solution; mixing a sodium alginate solution, a nano zinc oxide solution and a chitosan solution to obtain a composite material solution; and stirring and mixing the composite material solution at 38-42 DEG C for 12-18 minutes, and then preparing a thin film to obtain the sodium alginate / nano-zinc oxide composite adsorbent. The sodium alginate / nano-zinc oxide composite material is prepared by taking chitosan as a modifier and a mixed solution of hydrochloric acid and citric acid as a solvent, and has better adsorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a preparation method and application of a sodium alginate / nano zinc oxide composite adsorbent. Background Art

[0002] With the rapid development of industry in recent years, the treatment of heavy metals in wastewater has become a key content of environmental protection work. Sodium alginate raw materials are abundant and easy to obtain, and have low toxicity, good biocompatibility, film-forming property, thickening property, gel performance and high degradability. These unique properties make sodium alginate widely used in many fields. Sodium alginate has the advantages of being renewable, environmentally compatible, good film-forming property, abundant resources, easy to obtain and highly degradable. It has attracted more and more attention in many fields such as water treatment, cosmetics, and medicine. Its internal porous structure makes it a good adsorption material. Sodium alginate contains hydrophilic groups such as -COO- and -OH, which can be chelated and adsorbed with metal ions or some ionic dyes, but the adsorption effect of pure sodium alginate as an adsorbent is not ideal. Summary of the invention

[0003] The main purpose of the present invention is to propose a preparation method of a sodium alginate / nano zinc oxide composite adsorbent and its application, aiming to provide a method for preparing a sodium alginate / nano zinc oxide composite adsorbent.

[0004] To achieve the above object, the present invention provides a method for preparing a sodium alginate / nano zinc oxide composite adsorbent, comprising the following steps:

[0005] preparing a hydrochloric acid solution and a citric acid solution respectively, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution;

[0006] Using the mixed solution as a solvent to dissolve sodium alginate, nano zinc oxide and chitosan respectively to prepare a sodium alginate solution, a nano zinc oxide solution and a chitosan solution;

[0007] The sodium alginate solution, the nano zinc oxide solution and the chitosan solution are mixed to obtain a composite material solution;

[0008] The composite material solution is stirred and mixed at 38-42° C. for 12-18 minutes, and then prepared into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent.

[0009] Optionally, in the step of preparing a hydrochloric acid solution and a citric acid solution separately, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution:

[0010] The mass fraction of the hydrochloric acid solution is 1-3%, the mass fraction of the citric acid solution is 1-3%, and the volume ratio of the hydrochloric acid solution and the citric acid solution when mixed is 1:1.

[0011] Optionally, in the step of using the mixed solution as a solvent to dissolve sodium alginate, nano zinc oxide and chitosan respectively to prepare a sodium alginate solution, a nano zinc oxide solution and a chitosan solution:

[0012] The mass fraction of the sodium alginate solution is 1 to 3%; and / or,

[0013] The mass fraction of the nano zinc oxide solution is 1 to 10%; and / or,

[0014] The mass fraction of the chitosan solution is 1-3%.

[0015] Optionally, in the step of mixing the sodium alginate solution, the nano zinc oxide solution and the chitosan solution to obtain a composite material solution:

[0016] The total solid content of the composite material solution is 4-6%, wherein the total mass fraction of sodium alginate and nano zinc oxide is 1.5-2.5%, and the mass fraction of nano zinc oxide is 1-10% of the total solid content.

[0017] Optionally, in the step of mixing the sodium alginate solution, the nano zinc oxide solution and the chitosan solution to obtain a composite material solution:

[0018] The total solid content of the composite material solution is 5%, wherein the total mass fraction of sodium alginate and nano zinc oxide is 2%, and the mass fraction of nano zinc oxide is 1-10% of the total solid content.

[0019] Optionally, in the step of stirring and mixing the composite material solution at 38-42° C. for 12-18 minutes and then preparing it into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent:

[0020] The step of preparing the film comprises pouring the composite material solution into a mold and drying the solution to form a film.

[0021] Optionally, in the step of stirring and mixing the composite material solution at 38-42° C. for 12-18 minutes and then preparing it into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent:

[0022] The thickness of the film is 2-3 mm.

[0023] In addition, the present invention also proposes an application of a sodium alginate / nano-zinc oxide composite adsorbent in wastewater treatment. The sodium alginate / nano-zinc oxide composite adsorbent is prepared by the preparation method of the sodium alginate / nano-zinc oxide composite adsorbent as described above.

[0024] In the technical solution provided by the present invention, chitosan is used as a modifier and a mixed solution of hydrochloric acid and citric acid is used as a solvent to prepare a sodium alginate / nano zinc oxide composite material. The prepared composite adsorbent has better adsorption performance than sodium alginate, can be used as an adsorbent for treating wastewater and sewage, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 The present invention provides a schematic flow chart of an embodiment of a method for preparing a sodium alginate / nano zinc oxide composite adsorbent.

[0027] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0028] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.

[0029] Sodium alginate raw materials are abundant and easy to obtain, and have low toxicity, good biocompatibility, film-forming properties, thickening properties, gel properties and high degradability. These unique properties make sodium alginate widely used in many fields. Sodium alginate has the advantages of being renewable, environmentally compatible, good film-forming properties, abundant and easy to obtain resources and high degradability. It has attracted more and more attention in the fields of water treatment, cosmetics, medicine and many other fields. Its internal porous structure makes it a good adsorption material. Sodium alginate contains hydrophilic groups such as -COO- and -OH, which can be chelated and adsorbed with metal ions or some ionic dyes. Zinc oxide is a photocatalytic adsorption material. Under the action of light radiation, organic matter can be directly oxidized and decomposed by holes. At the same time, nano-sized ZnO has the characteristics of large specific surface area, high surface activity and strong adsorption capacity. The inventors have found through research that the adsorption effect of sodium alginate alone as an adsorbent is not ideal. After being combined with nano-zinc oxide, the adsorption performance of sodium alginate can be effectively improved. However, the sodium alginate / nano-zinc oxide composite has problems such as strong hydrophilicity, unsatisfactory mechanical properties, and poor dispersion effect of nano-zinc oxide.

[0030] Based on this, the inventors proposed a method for preparing a sodium alginate / nano zinc oxide composite adsorbent after in-depth research. The sodium alginate / nano zinc oxide composite material is prepared using chitosan as a modifier and a mixed solution of hydrochloric acid and citric acid as a solvent. Sodium alginate and nano zinc oxide are compounded by dissolving, dispersing and self-assembling to improve the performance of the material. Specifically, see Figure 1 As shown, an embodiment of the method for preparing the sodium alginate / nano zinc oxide composite adsorbent provided by the present invention comprises the following steps:

[0031] Step S10, preparing a hydrochloric acid solution and a citric acid solution respectively, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution;

[0032] Step S20, using the mixed solution as a solvent to dissolve sodium alginate, nano zinc oxide and chitosan respectively to prepare a sodium alginate solution, a nano zinc oxide solution and a chitosan solution;

[0033] Step S30, mixing the sodium alginate solution, the nano zinc oxide solution and the chitosan solution to obtain a composite material solution;

[0034] Step S40, stirring and mixing the composite material solution at 38-42° C. for 12-18 minutes, and then preparing it into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent.

[0035] First, a mixed solution of hydrochloric acid solution, citric acid solution and water of a certain concentration is prepared, and then the mixed solution is used as a solvent, and sodium alginate, nano zinc oxide and chitosan are dissolved respectively according to the principle of like dissolves like, so as to prepare sodium alginate solution, nano zinc oxide solution and chitosan solution of a certain concentration; the three solutions are then mixed to prepare a composite material solution; then, the composite material solution is stirred and mixed at a certain temperature, and in this process, the materials are fully dispersed and self-assembled; finally, the composite material solution after stirring and mixing is prepared into a film, so as to obtain the sodium alginate / nano zinc oxide composite adsorbent.

[0036] In the technical solution provided by the present invention, chitosan is used as a modifier, and a mixed solution of hydrochloric acid and citric acid is used as a solvent to prepare a sodium alginate / nano zinc oxide composite material. Chitosan and sodium alginate have a strong hydrogen bond effect, which can effectively improve the hydrophobicity and mechanical properties of the material. Hydrochloric acid and citric acid are used as solvents for nano zinc oxide of chitosan, so that the nano zinc oxide can be dispersed in the sodium alginate matrix in the form of ions, and the dispersion effect is better. The composite adsorbent finally prepared has better adsorption performance than sodium alginate, can be used as an adsorbent for treating wastewater and sewage, has good application prospects, and also lays a certain foundation for solving the application of sodium alginate composite materials.

[0037] In some embodiments of the present invention, the mass fraction of the hydrochloric acid solution in step S10 is 1-3%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, etc., preferably 2%; the mass fraction of the citric acid solution in step S10 is 1-3%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, etc., preferably 2%; the volume ratio of the hydrochloric acid solution and the citric acid solution when mixed in step S10 is 1:1. The mixed solution prepared by adding the ratio is used as a solvent for dissolving sodium alginate, nano zinc oxide and chitosan, and has good dissolution effect and high efficiency.

[0038] In some embodiments of the present invention, in some embodiments of the present invention, the mass fraction of the sodium alginate solution in step S20 is 1-3%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, etc., preferably 2%. The mass fraction of the nano zinc oxide solution in step S20 is 1-10%, for example, it can be 1%, 3%, 5%, 7%, 9%, 10%, etc. The mass fraction of the chitosan solution in step S20 is 1-3%, for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, etc., preferably 2%. By controlling the sodium alginate solution, nano zinc oxide solution and chitosan solution within the above mass fraction range, the solid matter is dissolved more fully and the solution preparation efficiency is higher.

[0039] In some embodiments of the present invention, the total solid content of the composite material solution in step S30 is 4-6%, for example, 4%, 4.5%, 5%, 5.5%, 6%, etc., wherein sodium alginate and nano-

[0040] The total mass fraction of zinc oxide is 1.5-2.5%, for example, 1.5%, 1.7%, 1.9%, 2.0%, 2.1%, 2.3%, 2.5%, etc., and the mass fraction of nano zinc oxide is 1-10% of the total solid content, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. By regulating the total solid content of the composite material solution and the addition amount of each solid component, it is beneficial to ensure that the final composite adsorbent has good adsorption performance, mechanical properties, hydrophobicity and dispersibility, and it is also convenient for the implementation of subsequent film preparation, molding and drying processes.

[0041] Further, in some preferred embodiments of the present invention, the total solid content of the composite material solution in step S30 is 5%, wherein the total mass fraction of sodium alginate and nano zinc oxide is 2%, and the mass fraction of nano zinc oxide is 1-10% of the total solid content. The total solid content of the composite material solution is controlled to be 5%, the total mass fraction of sodium alginate and nano zinc oxide is 2%, and the mass fraction of chitosan is 3%. In this way, the adsorption performance, mechanical properties and dispersibility of the prepared composite adsorbent all achieve better results.

[0042] There are many methods for preparing the composite material solution into a thin film, including but not limited to cast film, coating film, etc. In some embodiments of the present invention, the step of preparing the film in step S40 includes pouring the composite material solution into a mold and forming a film through drying. The process is simpler, the required equipment is simple, and the cost is low.

[0043] In some embodiments of the present invention, in step S40: the thickness of the film is 2-3 mm. Within this thickness range, the mechanical properties and adsorption properties of the sodium alginate / nano zinc oxide composite adsorbent are both better, and the drying rate of the film is also faster, which is conducive to simplifying the preparation process.

[0044] Based on the method provided by the present invention and the sodium alginate / nano zinc oxide composite adsorbent prepared therefrom, the present invention also proposes an application of the sodium alginate / nano zinc oxide composite adsorbent in wastewater treatment, and the preparation method of the sodium alginate / nano zinc oxide composite adsorbent refers to the above embodiment. The sodium alginate / nano zinc oxide composite adsorbent prepared by the method provided by the present invention is used for wastewater treatment, and the wastewater to be treated is filtered through the thin film-shaped sodium alginate / nano zinc oxide composite adsorbent to complete the wastewater treatment. The adsorption performance is good, and the heavy metals and other pollutants in the wastewater can be effectively adsorbed.

[0045] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0046] Example 1

[0047] (1) preparing a 2% by mass hydrochloric acid solution and a 2% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0048] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 2%, a nano zinc oxide solution with a mass fraction of 5% and a chitosan solution with a mass fraction of 2%;

[0049] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 5%, the mass fraction of nano zinc oxide is 1% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.05%), and the total mass fraction of sodium alginate and nano zinc oxide is 2%;

[0050] (4) The obtained composite material solution was stirred and mixed at 40° C. for 15 min, then poured into a mold and dried to form a film with a thickness of 2 mm, thereby obtaining a sodium alginate / nano zinc oxide composite adsorbent.

[0051] Example 2

[0052] (1) preparing a 2% by mass hydrochloric acid solution and a 2% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0053] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 2%, a nano zinc oxide solution with a mass fraction of 5% and a chitosan solution with a mass fraction of 2%;

[0054] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 5%, the mass fraction of nano zinc oxide is 3% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.15%), and the total mass fraction of sodium alginate and nano zinc oxide is 2%;

[0055] (4) The obtained composite material solution was stirred and mixed at 40° C. for 15 min, then poured into a mold and dried to form a film with a thickness of 2 mm to obtain a sodium alginate / nano zinc oxide composite adsorbent.

[0056] Example 3

[0057] (1) preparing a 2% by mass hydrochloric acid solution and a 2% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0058] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 2%, a nano zinc oxide solution with a mass fraction of 5% and a chitosan solution with a mass fraction of 2%;

[0059] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 5%, the mass fraction of nano zinc oxide is 5% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.25%), and the total mass fraction of sodium alginate and nano zinc oxide is 2%;

[0060] (4) The obtained composite material solution was stirred and mixed at 40° C. for 15 min, then poured into a mold and dried to form a film with a thickness of 2 mm to obtain a sodium alginate / nano zinc oxide composite adsorbent.

[0061] Example 4

[0062] (1) preparing a 2% by mass hydrochloric acid solution and a 2% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0063] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 2%, a nano zinc oxide solution with a mass fraction of 5% and a chitosan solution with a mass fraction of 2%;

[0064] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 5%, the mass fraction of nano zinc oxide is 10% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.5%), and the total mass fraction of sodium alginate and nano zinc oxide is 2%;

[0065] (4) The obtained composite material solution was stirred and mixed at 40° C. for 15 min, then poured into a mold and dried to form a film with a thickness of 2 mm, thereby obtaining a sodium alginate / nano zinc oxide composite adsorbent.

[0066] Example 5

[0067] (1) preparing a 3% by mass hydrochloric acid solution and a 3% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0068] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 1%, a nano zinc oxide solution with a mass fraction of 1%, and a chitosan solution with a mass fraction of 1%;

[0069] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 4%, the mass fraction of nano zinc oxide is 1% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.04%), and the total mass fraction of sodium alginate and nano zinc oxide is 1.5%;

[0070] (4) The obtained composite material solution was stirred and mixed at 38° C. for 18 min, then poured into a mold and dried to form a film with a thickness of 3 mm to obtain a sodium alginate / nano zinc oxide composite adsorbent.

[0071] Example 6

[0072] (1) preparing a 1% by mass hydrochloric acid solution and a 1% by mass citric acid solution respectively, and then mixing the prepared hydrochloric acid solution and the citric acid solution in a volume ratio of 1:1 to obtain a mixed solution;

[0073] (2) using the prepared mixed solution as a solvent, dissolving sodium alginate, nano zinc oxide and chitosan respectively, to prepare a sodium alginate solution with a mass fraction of 3%, a nano zinc oxide solution with a mass fraction of 10% and a chitosan solution with a mass fraction of 3%;

[0074] (3) mixing the prepared sodium alginate solution, nano zinc oxide solution and chitosan solution to obtain a composite material solution, wherein the total solid content of the composite material solution is controlled to be 6%, the mass fraction of nano zinc oxide is 1% of the total solid content (i.e., the mass fraction of nano zinc oxide in the composite material solution is 0.06%), and the total mass fraction of sodium alginate and nano zinc oxide is 2.5%;

[0075] (4) The obtained composite material solution was stirred and mixed at 42° C. for 12 minutes, then poured into a mold and dried to form a film with a thickness of 2.5 mm, thereby obtaining a sodium alginate / nano zinc oxide composite adsorbent.

[0076] The adsorption effects of the adsorbents prepared in the above embodiments were tested respectively, and the specific methods and results are as follows:

[0077] Adsorption experiment: First, mix 50mL of distilled water and 100mL of methyl orange solution, measure the pH with a pH meter, and then adjust the pH of the solution with hydrochloric acid solution or sodium hydroxide solution. At the same time, use a clean cuvette to measure the absorbance of the mixed solution (465nm) as the initial absorbance A0. Accurately weigh 0.1g of adsorbent, put the adsorbent into the prepared methyl orange solution, put in a stirring magnet, and finally place it in a dark box equipped with a magnetic stirrer and an ultraviolet lamp, adjust the stirring speed to a uniform level, control the temperature to 15°C (normal temperature without heating), and turn on the ultraviolet lamp for adsorption for a certain period of time. After the adsorption is completed, take the upper solution and add it to a centrifugal tube, and use a centrifuge to centrifuge at 3000rpm for 3min. After the centrifugation is completed, use a laboratory syringe to draw the upper clear liquid and add it to the cuvette, and measure the absorbance A of the solution at a wavelength of 465nm.

[0078] The adsorption rate calculation formula is: Q = (A0-A) / A0×100%, where Q represents the adsorption rate, A0 is the absorbance of the methyl orange solution before adsorption, and A is the absorbance of the methyl orange solution after the adsorption is completed.

[0079] The adsorption rate calculation results are shown in Table 1 below.

[0080] Table 1 Adsorption rate of the adsorbents prepared in each embodiment at different times

[0081]

[0082] As can be seen from Table 1, the sodium alginate / nano zinc oxide composite adsorbent prepared in the embodiment of the present invention adsorbs methyl orange very quickly. The experimental results show that the methyl orange concentration of the four groups of samples is greatly reduced within 15 minutes, and the adsorption rate is close to 80% during this period. The adsorption rate tends to be flat within the next 30 minutes. After 60 minutes of adsorption, the absorbance of the solution changes very little and reaches adsorption equilibrium, indicating that the composite adsorbent prepared by the present invention has good adsorption performance.

[0083] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A method for preparing a sodium alginate / nano zinc oxide composite adsorbent, characterized in that: The following steps are involved: preparing a hydrochloric acid solution and a citric acid solution respectively, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution; Using the mixed solution as a solvent to dissolve sodium alginate, nano zinc oxide and chitosan respectively to prepare a sodium alginate solution, a nano zinc oxide solution and a chitosan solution; The sodium alginate solution, the nano zinc oxide solution and the chitosan solution are mixed to obtain a composite material solution; The composite material solution is stirred and mixed at 38-42° C. for 12-18 minutes, and then prepared into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent.

2. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: In the step of preparing a hydrochloric acid solution and a citric acid solution respectively, and then mixing the hydrochloric acid solution and the citric acid solution to prepare a mixed solution: The mass fraction of the hydrochloric acid solution is 1-3%, the mass fraction of the citric acid solution is 1-3%, and the volume ratio of the hydrochloric acid solution and the citric acid solution when mixed is 1:

1.

3. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: In the step of using the mixed solution as a solvent to dissolve sodium alginate, nano zinc oxide and chitosan respectively to prepare a sodium alginate solution, a nano zinc oxide solution and a chitosan solution: The mass fraction of the sodium alginate solution is 1 to 3%; and / or, The mass fraction of the nano zinc oxide solution is 1 to 10%; and / or, The mass fraction of the chitosan solution is 1-3%.

4. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: In the step of mixing the sodium alginate solution, the nano zinc oxide solution and the chitosan solution to obtain a composite material solution: The total solid content of the composite material solution is 4-6%, wherein the total mass fraction of sodium alginate and nano zinc oxide is 1.5-2.5%, and the mass fraction of nano zinc oxide is 1-10% of the total solid content.

5. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: In the step of mixing the sodium alginate solution, the nano zinc oxide solution and the chitosan solution to obtain a composite material solution: The total solid content of the composite material solution is 5%, wherein the total mass fraction of sodium alginate and nano zinc oxide is 2%, and the mass fraction of nano zinc oxide is 1-10% of the total solid content.

6. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: The composite material solution is stirred and mixed at 38-42° C. for 12-18 minutes, and then prepared into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent: The step of preparing the film comprises pouring the composite material solution into a mold and drying the solution to form a film.

7. The method for preparing the sodium alginate / nano zinc oxide composite adsorbent according to claim 1, characterized in that: The composite material solution is stirred and mixed at 38-42° C. for 12-18 minutes, and then prepared into a film to obtain a sodium alginate / nano zinc oxide composite adsorbent: The thickness of the film is 2-3 mm.

8. Application of a sodium alginate / nano zinc oxide composite adsorbent in wastewater treatment, characterized in that: The sodium alginate / nano-zinc oxide composite adsorbent is prepared by the preparation method of the sodium alginate / nano-zinc oxide composite adsorbent according to any one of claims 1 to 7.