Preparation method of high-dispersity and high-loading-capacity carbon-loaded platinum and palladium noble metal catalyst
By forming functional group anchor points on the surface of activated carbon, the metal-support interaction is enhanced, and the problem of insufficient particle size and load capacity of existing carbon-supported precious metal catalysts is solved, and small-size and high-load carbon-supported precious metal catalysts are achieved, which significantly improves the Catalytic performance and service life.
Patent Information
- Application Number
- CN202411290476.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The precious metal particles of existing carbon-loaded precious metal catalysts have large diameters, uneven distribution, and insufficient load capacity, resulting in unsatisfactory catalytic efficiency and difficult to meet the needs of high load applications such as fuel cells.
By forming a conjugated structure with the surface of activated carbon by organic compounds such as benzoic acid, aniline, benzene thiol, 1-aminopyridine, etc., forming anchors of amino, thiol and carboxylic functional groups, enhancing metal-support interactions, and inhibiting the growth and agglomeration of precious metal nanoparticles. A carbon-supported precious metal catalyst is formed with small size and high loads.
The catalytic performance and service life of the catalyst are significantly improved. The diameter of precious metal particles is between 0.5-4 nanometers, and the dispersion is evenly distributed, with a load capacity of up to 70%. It is suitable for fuel cells and hydrogen production in water electrolytic.
Smart Images

Figure CN119056442A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation and noble metal catalysis, and relates to a method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst. Background Art
[0002] As a metal catalyst, precious metal catalysts are a type of precious metal catalytic material that can significantly change the rate of chemical reactions without participating in the final product of the reaction. Platinum and palladium-based catalysts are the most widely used. Because their d-electron orbits are not filled, these precious metals are easy to adsorb reactants on the surface, and have moderate strength, which is conducive to the formation of intermediate "active compounds". They have high catalytic activity and also have comprehensive excellent properties such as high temperature resistance, oxidation resistance, and corrosion resistance, making them the most important catalyst materials. At present, in the field of new energy, carbon-supported platinum, palladium, ruthenium and other precious metal supported catalysts have become the most critical part in the development of proton exchange membrane fuel cells, water electrolysis to produce hydrogen, and hydrogenation and dehydrogenation reactions.
[0003] However, in the prior art, carbon-supported noble metal catalysts are usually prepared by directly impregnating activated carbon into an alcohol or aqueous solution of a noble metal salt and then undergoing a thermal reduction method. The disadvantage of this process is that the interaction between the activated carbon itself and the noble metal is weak, so the anchoring effect on the noble metal nanoparticles in the catalyst is not strong, resulting in a large particle diameter of the noble metal in the catalyst during the preparation process, resulting in a low specific surface area of the catalyst and unsatisfactory catalytic efficiency. In addition, the noble metal loading in the prior art is generally below 40%, which is difficult to meet the application needs of high metal loading in fuel cell catalysts.
[0004] Therefore, there is an urgent need to explore a catalyst with small precious metal particle size, uniform size distribution, and high loading capacity to solve the above technical problems. Summary of the invention
[0005] In order to solve the above problems, the present invention forms a conjugated structure through the conjugated π bonds in benzoic acid, aniline, benzenethiol, and 1-aminopyridine molecules and the localized graphitized units on the activated carbon, thereby forming anchor points containing amino (-NH2), thiol (-SH) and carboxyl (-COOH) functional groups on the surface of the activated carbon. In the subsequent polyol reduction process, these anchor points can significantly improve the interaction between the metal and the carrier, thereby inhibiting the growth and agglomeration of metal nanoparticles on the surface of the activated carbon, and then easily forming a small-sized, high-load carbon-supported precious metal catalyst, which significantly improves the catalytic performance and service life of the catalyst.
[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst, comprising the following steps:
[0007] Step 1, mixing the functional organic compound and methanol in a mass ratio of 1:8-12, and uniformly dispersing by ultrasonication to obtain a mixed solution A;
[0008] The carbon carrier is added to the mixed solution A, wherein the mass ratio of the carbon carrier to the mixed solution is 1:8-12, the mixed solution is ultrasonically treated for 50-70 minutes, then stirred and refluxed at 55-65° C. for 8-12 hours, and finally filtered, washed and dried to obtain surface functionalized activated carbon powder B.
[0009] Step 2, mixing NaOH and ethylene glycol in a mass ratio of 1:90-110, and stirring sufficiently to obtain a mixed solution C;
[0010] Step 3, adding Pt salt or Pd salt and activated carbon powder B to a mixed solution C, wherein the mass ratio of Pt metal in the Pt salt or Pd metal in the Pd salt to the activated carbon powder B is 1-30:12; the mass ratio of the total mass of the Pt salt or Pd salt and the activated carbon powder B to the mixed solution C is 1:900-1100, stirring and reflux the obtained mixed solution at 150-170°C for 3-5 hours, and after the solution is cooled to room temperature, heating with H 2 SO 4 After adjusting the pH to 3.9-4.1, continue stirring for 10-14 hours, and finally filter the reactant, wash it with ethanol, and dry it to obtain catalyst precursor powder D;
[0011] Step 4, grinding the catalyst precursor powder D and placing it in a muffle furnace for heat treatment at 380-420° C. for 50-70 minutes to obtain a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst.
[0012] Preferably, in step 1, the functional organic compound includes: benzoic acid, aniline, benzenethiol, and 1-aminopyridine.
[0013] Preferably, in step 1, the functional organic compound and methanol are mixed in a mass ratio of 1:10.
[0014] Preferably, in step 1, the carbon carrier includes: commercial activated carbon Vulcan XC-72, carbon black, and Ketjen black.
[0015] Preferably, in step 1, the mass ratio of the carbon carrier to the mixed solution A is 1:10, the mixed solution is ultrasonically treated for 60 minutes, and then stirred and refluxed at 60° C. for 10 hours.
[0016] Preferably, in step 3, the Pt salt comprises: chloroplatinic acid H 2 PtCl 6 , Potassium chloroplatinite K 2 PtCl 4, platinum acetylacetonate; the Pd salts include: palladium acetate, palladium nitrate, and palladium acetylacetonate.
[0017] Preferably, in step 3, the mass ratio of the Pt metal in the Pt salt or the Pd metal in the Pd salt to the activated carbon powder B is 3-28:12.
[0018] Preferably, in step 4, the catalyst precursor powder D is heat treated at a temperature of 400° C. for 60 minutes.
[0019] The beneficial effects of the present invention are:
[0020] 1. The present invention uses benzoic acid, aniline, benzenethiol, and 1-aminopyridine to perform surface functionalization on an activated carbon carrier. The carboxyl, amino, and thiol functional groups in these organic small molecule compounds can form anchor points on the activated carbon carrier. These anchor points can anchor the formed catalyst nanoparticles in the subsequent alcohol thermal reduction of precious metal ions, strengthen the metal-carrier interaction, and then inhibit the growth and agglomeration of the nanoparticles in the subsequent process, so that the nanoparticles are evenly dispersed on the carbon carrier, forming a small-sized, high-load carbon-supported precious metal catalyst, which significantly improves the catalytic performance and service life of the catalyst.
[0021] 2. The present invention places the prepared catalyst precursor powder in a muffle furnace and heat treats it at 400°C to remove excess small molecule organic compounds on the surface of the carbon carrier, while further strengthening the interaction between the metal and the carrier, which helps to improve the stability of the catalyst.
[0022] 3. The present invention does not require additional equipment during the preparation process, and the preparation method is simple, has low equipment requirements, good repeatability, and is easy to realize industrial production.
[0023] 4. The diameter of the precious metal particles of the catalyst obtained by the present invention is between 0.5 and 4 nanometers, the particles are evenly dispersed, the size is uniform and there is no agglomeration, and the precious metal loading can reach up to 70%. It has broad application prospects in related fields such as fuel cells and water electrolysis hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a transmission electron microscope image of a carbon-supported Pt catalyst with a noble metal loading of 20% prepared in Example 1 of the method for preparing a high-dispersion and high-loading carbon-supported platinum and palladium noble metal catalyst of the present invention;
[0025] Figure 2 is a transmission electron microscope image of a carbon-supported Pt catalyst with a noble metal loading of 40% prepared in Example 2 of the present invention;
[0026] Figure 3is a transmission electron microscope image of a carbon-supported Pt catalyst with a noble metal loading of 70% prepared in Example 3 of the present invention;
[0027] Figure 4 is a transmission electron microscope image of a carbon-supported Pd catalyst with a noble metal loading of 30% prepared in Example 4 of the present invention;
[0028] Figure 5 is a transmission electron microscope image of a carbon-supported Pd catalyst with a noble metal loading of 50% prepared in Example 5 of the present invention;
[0029] Figure 6 It is a transmission electron microscope image and size distribution diagram of the carbon-supported Pd catalyst with a carbon noble metal loading of 60% prepared in Example 6 of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the relevant technologies in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] refer to Figures 1 to 6 The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst in this embodiment comprises the following steps:
[0032] Step 1, mixing one of the functional organic compounds (benzoic acid, aniline, benzenethiol, 1-aminopyridine) and methanol in a mass ratio of 1:10, and uniformly dispersing by ultrasonication to obtain a mixed solution A; adding one of the carbon carrier commercial activated carbon Vulcan XC-72, carbon black or Ketjen black to the mixed solution A, wherein the mass ratio of activated carbon to the mixed solution is 1:10, ultrasonically treating for 60 minutes, and then stirring and refluxing at 60°C for 10 hours, and finally filtering, washing, and drying to obtain a surface functionalized activated carbon powder B.
[0033] Step 2, mixing NaOH and ethylene glycol at a mass ratio of 1:100, and stirring thoroughly to obtain a mixed solution C;
[0034] Step 3, adding Pt salt or Pd salt and activated carbon powder B to a mixed solution C, wherein the mass ratio of Pt or Pd metal in the Pt salt or Pd salt to the activated carbon powder B is 3-28:12; the mass ratio of the total mass of the Pt salt or Pd salt and the activated carbon powder B to the C solution is 1:1000, stirring and reflux the obtained mixed solution at 160°C for 4 hours, and after the solution is cooled to room temperature, heating with H 2 SO 4After adjusting the pH to 4, stirring was continued for 12 hours, and finally the reactant was filtered, washed with ethanol, and dried to obtain catalyst precursor powder D;
[0035] Step 4, grinding the catalyst precursor powder D and placing it in a muffle furnace, and heat treating it at 400° C. for 60 minutes to obtain a carbon-supported platinum and palladium noble metal catalyst with high dispersion and high loading.
[0036] Example
[0037] The present invention will be further described below by means of specific examples.
[0038] Embodiment 1:
[0039] Benzoic acid was dissolved in methanol at a mass ratio of 1:10, and ultrasonicated for 10 minutes to make it evenly dispersed. Then, commercial activated carbon black and the mixed solution were mixed at a mass ratio of 1:10, ultrasonicated for 60 minutes, and then stirred and refluxed at 60°C for 10 hours. Finally, the activated carbon powder with benzoic acid surface functionalization was obtained by filtering, washing and drying. NaOH and ethylene glycol were mixed at a mass ratio of 1:100 and stirred for 10 minutes. After NaOH was fully dissolved, an ethylene glycol alkaline solution was obtained. Then, according to the mass ratio of precious metal Pt to surface functionalized activated carbon powder of 3:12, chloroplatinic acid and surface functionalized activated carbon powder were added in sequence, so that the total mass of chloroplatinic acid plus surface functionalized activated carbon powder and the mass ratio of ethylene glycol alkaline solution were 1:1000. The resulting mixed solution was stirred and refluxed at 160°C for 4 hours. After the solution was cooled to room temperature, H 2 SO 4 After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pt catalyst with a precious metal Pt content of about 20%.
[0040] Figure 1 This is the transmission electron microscopy image of the prepared sample. The Pt nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 1.2nm. The particles are evenly distributed without obvious agglomeration.
[0041] Embodiment 2:
[0042] Aniline was dissolved in methanol at a mass ratio of 1:10, and ultrasonicated for 10 minutes to make it evenly dispersed. Then, commercial activated carbon Vulcan XC-72 was mixed with the mixed solution at a mass ratio of 1:10, ultrasonicated for 60 minutes, and then stirred and refluxed at 60°C for 10 hours. Finally, activated carbon powder with aniline surface functionalization was obtained by filtering, washing and drying. NaOH and ethylene glycol were mixed at a mass ratio of 1:100 and stirred for 10 minutes. After NaOH was fully dissolved, an ethylene glycol alkaline solution was obtained. Then, chloroplatinic acid and surface functionalized activated carbon Vulcan XC-72 were added in sequence according to the mass ratio of precious metal Pt to surface functionalized activated carbon powder of 12:12, so that the total mass of chloroplatinic acid plus surface functionalized activated carbon powder and the mass ratio of ethylene glycol alkaline solution was 1:1000. The resulting mixed solution was stirred and refluxed at 160°C for 4 hours. After the solution was cooled to room temperature, H 2 SO 4 After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pt catalyst with a precious metal Pt content of about 40%.
[0043] Figure 2 This is the transmission electron microscopy image of the prepared sample. The Pt nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 2.2nm. The particles are evenly distributed without obvious agglomeration.
[0044] Embodiment 3:
[0045] Dissolve benzenethiol in methanol at a mass ratio of 1:10, and ultrasonicate for 10 minutes to make it evenly dispersed. Then, mix the commercial activated carbon Ketjen black with the mixed solution at a mass ratio of 1:10, ultrasonicate for 60 minutes, and then stir and reflux at 60°C for 10 hours. Finally, filter, wash and dry to obtain activated carbon powder with benzenethiol surface functionalization. Mix NaOH and ethylene glycol at a mass ratio of 1:100 and stir well for 10 minutes. After NaOH is fully dissolved, an ethylene glycol alkaline solution is obtained. Then, potassium chloroplatinite and surface functionalized activated carbon Ketjen black are added in sequence according to the mass ratio of precious metal Pt to surface functionalized activated carbon powder of 28:12, so that the total mass of potassium chloroplatinite plus surface functionalized activated carbon powder and the mass ratio of ethylene glycol alkaline solution are 1:1000. The resulting mixed solution is stirred and refluxed at 160°C for 4 hours. After the solution is cooled to room temperature, it is treated with H 2 SO 4After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pt catalyst with a precious metal Pt content of about 70%.
[0046] Figure 3 This is the transmission electron microscopy image of the prepared sample. The Pt nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 2.8nm. The particles are evenly distributed without obvious agglomeration.
[0047] Embodiment 4:
[0048] Benzoic acid was dissolved in methanol at a mass ratio of 1:10, and ultrasonicated for 10 minutes to make it evenly dispersed. Then, commercial activated carbon Ketchen black was mixed with the mixed solution at a mass ratio of 1:10, ultrasonicated for 60 minutes, and then stirred and refluxed at 60°C for 10 hours. Finally, activated carbon powder with benzoic acid surface functionalization was obtained by filtering, washing and drying. NaOH and ethylene glycol were mixed at a mass ratio of 1:100 and stirred for 10 minutes. After NaOH was fully dissolved, an ethylene glycol alkaline solution was obtained. Then, palladium acetate and surface functionalized activated carbon Ketchen black were added in sequence at a mass ratio of 6:12 between the precious metal Pd and the surface functionalized activated carbon powder, so that the total mass of palladium acetate plus the surface functionalized activated carbon powder and the mass ratio of the ethylene glycol alkaline solution was 1:1000. The resulting mixed solution was stirred and refluxed at 160°C for 4 hours. After the solution was cooled to room temperature, H 2 SO 4 After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pd catalyst with a precious metal Pd content of about 30%.
[0049] Figure 4 This is the transmission electron microscopy image of the prepared sample. The Pd nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 3nm. The particles are evenly distributed without obvious agglomeration.
[0050] Embodiment 5:
[0051] 1-Aminopyridine was dissolved in methanol at a mass ratio of 1:10, and ultrasonicated for 10 minutes to make it evenly dispersed. Then, commercial activated carbon black and the mixed solution were mixed at a mass ratio of 1:10, ultrasonicated for 60 minutes, and then stirred and refluxed at 60°C for 10 hours. Finally, 1-aminopyridine surface functionalized activated carbon powder was obtained by filtering, washing and drying. NaOH and ethylene glycol were mixed at a mass ratio of 1:100 and stirred for 10 minutes. After NaOH was fully dissolved, an ethylene glycol alkaline solution was obtained. Then, acetylacetonate palladium and surface functionalized activated carbon black were added in sequence in a ratio of 12:12 between the precious metal Pd and the surface functionalized activated carbon powder, so that the total mass of acetylacetonate palladium plus the surface functionalized activated carbon powder and the mass ratio of the ethylene glycol alkaline solution was 1:1000. The resulting mixed solution was stirred and refluxed at 160°C for 4 hours. After the solution was cooled to room temperature, H 2 SO 4 After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pd catalyst with a precious metal Pd content of about 50%.
[0052] Figure 5 This is the transmission electron microscopy image of the prepared sample. The Pd nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 3.8nm. The particles are evenly distributed without obvious agglomeration.
[0053] Embodiment 6:
[0054] Dissolve benzenethiol in methanol at a mass ratio of 1:10, and ultrasonicate for 10 minutes to make it evenly dispersed. Then, commercial activated carbon Ketjen black and the mixed solution were mixed at a mass ratio of 1:10, ultrasonicated for 60 minutes, and then stirred and refluxed at 60°C for 10 hours. Finally, after filtering, washing and drying, activated carbon powder with benzenethiol surface functionalization was obtained. NaOH and ethylene glycol were mixed at a mass ratio of 1:100 and stirred for 10 minutes. After NaOH was fully dissolved, an ethylene glycol alkaline solution was obtained. Then, palladium nitrate and surface functionalized activated carbon Ketjen black were added in sequence in a ratio of 18:12 between the precious metal Pd and the surface functionalized activated carbon powder, so that the total mass of palladium nitrate plus the surface functionalized activated carbon powder and the mass ratio of the ethylene glycol alkaline solution was 1:1000. The resulting mixed solution was stirred and refluxed at 160°C for 4 hours. After the solution was cooled to room temperature, H 2 SO 4 After adjusting the pH to 4, continue stirring for 12 hours. Finally, filter the reactant, wash it with ethanol, dry it, grind it, place it in a muffle furnace, and heat treat it at 400°C for 60 minutes to obtain a highly dispersed carbon-supported Pd catalyst with a precious metal Pd content of about 60%.
[0055] Figure 6 This is the transmission electron microscopy image of the prepared sample. The Pd nanoparticles are evenly dispersed on the carrier carbon black. The average particle size is 4.3nm. The particles are evenly distributed without obvious agglomeration.
[0056] This specific implementation method uses organic small molecules containing amino, carboxyl, thiol and other functional groups to modify the surface of activated carbon to form anchor points. The anchoring effect of these functional groups on precious metal nanoparticles is utilized to strengthen the metal-carrier interaction and the excessive growth of precious metal ions during the reduction and nucleation process, and finally form a small-sized, highly dispersed and highly loaded carbon-supported precious metal catalyst. This method is an improvement on the traditional impregnation + alcohol thermal reduction method, so no additional equipment is required, and the preparation method is simple, the equipment requirements are low, and it is easy to realize industrial production. The diameter of the precious metal particles of the catalyst obtained by the present invention is between 0.5-4 nanometers, the particles are evenly dispersed, the size is uniform and there is no agglomeration, and the precious metal loading can reach up to 70%.
[0057] In summary, the present invention uses benzoic acid, aniline, benzenethiol, and 1-aminopyridine to functionalize the surface of the activated carbon carrier, wherein the carboxyl, amino, and thiol functional groups in these organic small molecule compounds can form anchor points on the activated carbon carrier, and these anchor points can anchor the formed catalyst nanoparticles during the subsequent alcohol thermal reduction of precious metal ions, thereby strengthening the metal-carrier interaction, thereby inhibiting the growth and agglomeration of the nanoparticles in the subsequent process, making them uniformly dispersed on the carbon carrier, forming a small-sized, high-loaded carbon-supported precious metal catalyst, and significantly improving the catalytic performance and service life of the catalyst.
[0058] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst, characterized in that: The following steps are involved: Step 1, mixing the functional organic compound and methanol in a mass ratio of 1:8-12, and uniformly dispersing by ultrasonication to obtain a mixed solution A; The carbon carrier is added to the mixed solution A, wherein the mass ratio of the carbon carrier to the mixed solution is 1:8-12, the mixed solution is subjected to ultrasonic treatment for 50-70 minutes, and then stirred and refluxed at 55-65° C. for 8-12 hours, and finally filtered, washed, and dried to obtain a surface functionalized activated carbon powder B; Step 2, mixing NaOH and ethylene glycol in a mass ratio of 1:90-110, and stirring sufficiently to obtain a mixed solution C; Step 3, adding Pt salt or Pd salt and activated carbon powder B to a mixed solution C, wherein the mass ratio of Pt metal in the Pt salt or Pd metal in the Pd salt to the mass ratio of activated carbon powder B is 1-30:12; the mass ratio of the total mass of the Pt salt or Pd salt and activated carbon powder B to the mixed solution C is 1:900-1100, stirring and refluxing the obtained mixed solution at 150-170° C. for 3-5 hours, after the solution is cooled to room temperature, adjusting the pH to 3.9-4.1 with H2SO4, continuing stirring for 10-14 hours, and finally filtering the reactant, washing with ethanol, and drying to obtain a catalyst precursor powder D; Step 4, grinding the catalyst precursor powder D and heat treating it at 380-420° C. for 50-70 minutes to obtain a carbon-supported platinum and palladium noble metal catalyst with high dispersion and high loading.
2. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 1, the functional organic compound includes: benzoic acid, aniline, benzenethiol, and 1-aminopyridine.
3. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 1, the functional organic compound and methanol are mixed in a mass ratio of 1:
10.
4. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 1, the carbon carrier includes: commercial activated carbon Vulcan XC-72, carbon black, and Ketjen black.
5. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 1, the mass ratio of the carbon carrier to the mixed solution A is 1:10, the mixed solution is ultrasonically treated for 60 minutes, and then stirred and refluxed at 60° C. for 10 hours.
6. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In step 3, the Pt salt includes: chloroplatinic acid H2PtCl6, potassium chloroplatinite K2PtCl4, platinum acetylacetonate; the Pd salt includes: palladium acetate, palladium nitrate, palladium acetylacetonate.
7. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 3, the mass ratio of the Pt metal in the Pt salt or the Pd metal in the Pd salt to the activated carbon powder B is 3-28:
12.
8. The method for preparing a high-dispersion and high-load carbon-supported platinum and palladium noble metal catalyst according to claim 1, characterized in that: In the step 4, the catalyst precursor powder D is heat treated at a temperature of 400° C. for 60 minutes.
Citation Information
Patent Citations
Loading type Pd base metal nanometer cluster catalyst, preparing method and applications thereof
CN101767018A
Method for improving stability of fuel cell catalyst and utilization rate of catalyst
CN102024965A
Preparation method of supported nano palladium / carbon catalyst
CN103933973A
Catalyst nanoparticle
US20080050641A1
KR20220039993A