Moisture-proof manganese-based catalyst as well as preparation method and application thereof

By preparing a moisture-resistant FeMn catalyst, the problem of manganese-based catalysts being easily deactivated under high humidity is solved, efficient ozone decomposition and catalyst life extension are achieved, and are suitable for industrial ozone removal.

CN119056465APending Publication Date: 2024-12-03WUXI WEIFU ENVIRONMENT PROTECTION CATALYST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207952.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing manganese-based catalysts are prone to absorb and inactivate water in high humidity environments, affecting the ozone decomposition efficiency and catalyst life.

Method used

Iron salt, manganese salt and organic anionic compounds are dissolved in deionized water, pH value is adjusted, and FeMn catalyst is prepared after crystallization and calcination to improve its moisture resistance.

Benefits of technology

The prepared wet-resistant manganese-based catalyst maintains high conversion and stability under high humidity, and extends the catalytic ozone decomposition life, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056465A_ABST
    Figure CN119056465A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ozonolysis, and particularly relates to a moisture-proof manganese-based catalyst as well as a preparation method and application thereof. The preparation method of the moisture-proof manganese-based catalyst comprises the following steps: dissolving ferric salt, manganese salt and an organic anionic compound in deionized water without CO2, dropwise adding a NaOH solution without CO2 into the deionized water under the protection of N2, enabling the pH value of the solution to be 8-11, stirring for 2-6 hours, transferring the mixed solution into a crystallization kettle, and crystallizing for 6-24 hours at 90-150 DEG C; and after cooling, carrying out centrifugal separation, washing with deionized water for multiple times until the solution is neutral, and roasting at 150-300 DEG C for 12-24 hours to obtain the FeMn ozone decomposition catalyst with moisture resistance. According to the moisture-resistant manganese-based catalyst prepared by the preparation method disclosed by the invention, the moisture resistance of the catalyst can be effectively improved in a high-humidity ozonolysis reaction, so that the catalytic life of the manganese-based catalyst is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ozone decomposition, and specifically relates to a moisture-resistant manganese-based catalyst and a preparation method and application thereof. Background Art

[0002] Ozone is a common air pollutant. Long-term exposure to ozone as low as 50-80ppb will affect human health. In the fields of industrial wastewater, waste gas treatment units and civil purifiers, the exhaust gas often contains a certain concentration of ozone, which needs to be removed before it can be discharged. Removing ozone is crucial for our health, ecological civilization construction and sustainable development strategy.

[0003] At present, the main methods for removing ozone include thermal decomposition, activated carbon adsorption, liquid absorption, electromagnetic wave radiation decomposition, etc., but they generally have problems such as high energy consumption and secondary pollution. Room temperature catalytic decomposition is recognized as the most promising and application-oriented ozone decomposition method. The key to this technology lies in the preparation of high-performance catalysts.

[0004] Manganese-based catalysts show high activity in catalytic ozone decomposition at room temperature, and their catalytic activity depends on the content and properties of oxygen vacancies on the catalyst surface. In the ozone decomposition process, in addition to the properties of the catalyst itself, some external conditions will also affect the activity of the catalyst in decomposing ozone, among which humidity has the greatest impact. If the oxygen vacancies in the reaction are occupied by water molecules, the catalyst will be deactivated. Summary of the invention

[0005] In order to solve the problem that the ozone decomposition catalyst is easily deactivated by water absorption, the present invention prepares a moisture-resistant manganese-based catalyst and its preparation method and application. The moisture-resistant manganese-based catalyst prepared by the present invention reduces the adsorption of water molecules on the active site in the ozone decomposition reaction at high humidity, can effectively improve the moisture resistance of the catalyst, and effectively prolongs the catalytic life of the manganese-based catalyst.

[0006] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is: In a first aspect, an embodiment of the present invention provides a method for preparing a moisture-resistant manganese-based catalyst, comprising the following steps: The iron salt, manganese salt and organic anion compound are dissolved in deionized water from which CO2 has been removed. Under the protection of N2, a NaOH solution from which CO2 has been removed is added dropwise thereto to adjust the pH value of the solution to 8-11. After stirring for 2-6 hours, the mixed solution is transferred to a crystallization kettle and crystallized at 90-150°C for 6-24 hours. After cooling, the mixture is separated by centrifugation and washed with deionized water for several times until it is neutral. After calcining at 150-300°C for 12-24 hours, a FeMn ozone decomposition catalyst with moisture resistance is obtained.

[0007] Furthermore, the iron salt Fe 3+ 、Mn in manganese salts 2+ The molar ratio of the organic anion compound to the organic anion compound is 1:1~5:0.5~3.

[0008] Further, the iron salt is one or more of ferric chloride, ferric sulfate, and ferric nitrate; The manganese salt is one or more of manganese chloride, manganese sulfate and manganese nitrate.

[0009] Furthermore, the organic anion compound is one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.

[0010] In a second aspect, an embodiment of the present invention provides a moisture-resistant manganese-based catalyst, which is prepared using the preparation method described in the first aspect.

[0011] In a third aspect, an embodiment of the present invention provides an application of the moisture-resistant manganese-based catalyst described in the second aspect, wherein the catalyst is used to catalyze an ozone decomposition reaction.

[0012] The technical solution provided by the embodiment of the present invention has the following beneficial effects: The FeMn ozone decomposition catalyst prepared by the present invention exhibits good moisture resistance in the ozone decomposition reaction, can achieve complete removal of ozone in high-humidity ozone decomposition, and has high stability.

[0013] The catalyst prepared by the present invention exhibits excellent moisture resistance in catalytic ozone decomposition. In a high humidity environment with a relative humidity of 80% at room temperature, the catalytic ozone decomposition is performed for 100 h, and the conversion rate is still maintained at above 99%. The life of the catalyst is effectively extended, providing a guarantee for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic diagram of the state of the catalyst prepared in Example 1 after coating the honeycomb carrier in water.

[0015] Figure 2 This is a schematic diagram of the state of the catalyst prepared in Example 1 after being coated on a honeycomb carrier in water.

[0016] Figure 3 The results are as follows for the conversion rates of ozone decomposition using the catalysts prepared in Example 1, Example 2, Example 3 and Comparative Example 1. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0018] Example 1 A method for preparing a moisture-resistant manganese-based catalyst comprises the following steps: Ferric chloride, manganese chloride and sodium dodecyl sulfate were dissolved in deionized water (Fe 3+ , Mn 2+ , sodium dodecyl sulfate in a molar ratio of 1:4:2), under the protection of N2, a 2 mol / L NaOH solution for removing CO2 was added dropwise thereto, the pH value of the solution was adjusted to 9, and after stirring for 2 h, the mixed solution was transferred to a crystallization kettle and crystallized at 110°C for 24 h; after cooling, it was separated by centrifugation, washed with deionized water for several times until neutral, and calcined at 250°C for 12 h to obtain a FeMn ozone decomposition catalyst with moisture resistance.

[0019] Example 2 A method for preparing a moisture-resistant manganese-based catalyst comprises the following steps: Ferric nitrate, manganese nitrate and sodium dodecylbenzene sulfonate were dissolved in deionized water (Fe 3+ , Mn 2+ , sodium dodecylbenzenesulfonate in a molar ratio of 1:3:0.5), under the protection of N2, a 2 mol / L NaOH solution for removing CO2 was added dropwise thereto, the pH value of the solution was adjusted to 10, and after stirring for 4 h, the mixed solution was transferred to a crystallization kettle and crystallized at 130°C for 12 h; after cooling, it was separated by centrifugation and washed with deionized water for several times until neutral, and calcined at 150°C for 24 h to obtain a FeMn ozone decomposition catalyst with moisture resistance.

[0020] Example 3 A method for preparing a moisture-resistant manganese-based catalyst comprises the following steps: Iron sulfate, manganese sulfate and sodium dodecyl sulfate were dissolved in deionized water (Fe 3+ , Mn 2+ , sodium dodecylbenzenesulfonate in a molar ratio of 1:2:1), under the protection of N2, a 2 mol / L NaOH solution for removing CO2 was added dropwise thereto, the pH value of the solution was adjusted to 8, and after stirring for 5 h, the mixed solution was transferred to a crystallization kettle and crystallized at 120°C for 18 h; after cooling, it was separated by centrifugation and washed with deionized water for several times until neutral, and calcined at 200°C for 18 h to obtain a FeMn ozone decomposition catalyst with moisture resistance.

[0021] Comparative Example 1 A method for preparing a manganese-based catalyst comprises the following steps: Dissolve ferric chloride and manganese chloride in deionized water (Fe 3+ , Mn 2+The molar ratio of the catalyst is 1:4), and under the protection of N2, a 2 mol / L NaOH solution for removing CO2 is added dropwise thereto, and the pH value of the solution is adjusted to 9. After stirring for 2 h, the mixed solution is transferred to a crystallization kettle and crystallized at 110°C for 24 h. After cooling, the mixture is separated by centrifugation and washed with deionized water for several times until it is neutral. After calcination at 250°C for 12 h, a FeMn ozone decomposition catalyst is obtained.

[0022] The catalysts prepared in Example 1, Example 2, Example 3 and Comparative Example 1 were applied to the ozone decomposition reaction. The specific operation was as follows: 10 g of catalyst, 10 g of aluminum gel with a mass fraction of 5% and 80 g of water were mixed to form a slurry, which was evenly coated on a cylindrical honeycomb carrier of the same specification, dried to remove water, and the catalyst coating amount was 100 g / L. Ozone decomposition test conditions: original ozone concentration 1 ppm, test temperature 25°C, relative humidity 80%, reaction space velocity 100000 h -1 Ozone conversion rate / %= (original ozone concentration - tail gas ozone concentration) / original ozone concentration 100%.

[0023] Figure 1 and Figure 2 Schematic diagrams of the states of the catalysts prepared in Example 1 and Comparative Example 1 in water after being coated on a honeycomb carrier. It can be seen that the catalyst coated in Example 1 floats on the water surface, indicating that it is hydrophobic, while the catalyst coated in Comparative Example 1 directly sinks into the water.

[0024] Figure 3 The results are the conversion results of the catalysts prepared in Example 1, Example 2, Example 3 and Comparative Example 1 in Example 4 when applied to ozone decomposition. Compared with Comparative Example 1, the FeMn catalysts prepared in Example 1, Example 2 and Example 3 showed higher conversion rates and better moisture resistance in the ozone decomposition reaction at high humidity, wherein the catalyst prepared in Example 1 catalyzed ozone decomposition for 100 h with a conversion rate of 100%, while the catalyst prepared in Comparative Example 1 had a reduced ozone conversion rate after 28 h of reaction, and the downward trend was obvious.

[0025] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a moisture-resistant manganese-based catalyst, It is characterized in that The following steps are involved: Dissolve iron salts, manganese salts and organic anion compounds in the CO removal 2 In deionized water, N 2 Under protection, CO is removed by dropping 2 of NaOH solution to make the solution pH = 8-11, after stirring for 2-6 hours, transfer the mixed solution into a crystallization kettle and crystallize at 90-150°C for 6-24 hours; after cooling, centrifuge and wash with deionized water several times until neutral, calcine at 150-300°C for 12-24 hours to obtain a moisture-resistant FeMn ozone decomposition catalyst.

2. The method for preparing the moisture-resistant manganese-based catalyst according to claim 1, It is characterized in that The iron salt Fe 3+ 、Mn in manganese salts 2+ The molar ratio of the organic anion compound to the organic anion compound is 1:1~5:0.5~3.

3. The method for preparing the moisture-resistant manganese-based catalyst according to claim 1 or 2, It is characterized in that The iron salt is one or more of ferric chloride, ferric sulfate, and ferric nitrate; The manganese salt is one or more of manganese chloride, manganese sulfate and manganese nitrate.

4. The method for preparing the moisture-resistant manganese-based catalyst according to claim 1, It is characterized in that The organic anion compound is one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.

5. A moisture-resistant manganese-based catalyst, It is characterized in that The method is prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the moisture-resistant manganese-based catalyst according to claim 5, It is characterized in that The catalyst is used for catalyzing ozone decomposition reaction.