Preparation method and application of high surface area Ag / Ca3 (PO4) 2 catalyst with hydrophobic surface

By preparing a high surface area Ag/Ca3(PO4)2 catalyst on a hydrophobic surface, the conversion rate of the catalyst in the oxidative dehydrogenation reaction of methoxypropanol is solved by using calcium phosphate support and silver ion formulation, combined with tetraethoxysilane coating. 低和选择性低的问题,实现了高效的甲氧基丙酮合成,催化剂寿命延长。

CN119056474APending Publication Date: 2024-12-03LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213773.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing catalysts have low conversion rate, low selectivity and short catalyst life in the oxidative dehydrogenation reaction of methoxypropanol, and are troubled by strong acidity, resulting in side reactions.

Method used

Using a high surface area Ag/Ca3(PO4)2 catalyst on a hydrophobic surface, prepared by an improved coprecipitation method, using calcium phosphate as a support for acid-base preparation, and a tetraethoxysilane is coated on the catalyst surface to reduce Hydrolysis reaction improves catalytic activity and selectivity.

Benefits of technology

The conversion rate of methoxypropanol and the selectivity of methoxyacetone were significantly improved, and the catalyst operated stably for 150 hours, which was far better than the performance of traditional catalysts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a high-surface-area Ag / Ca3 (PO4) 2 catalyst with a hydrophobic surface, which comprises the following steps: dropwise adding a calcium nitrate solution and a diammonium hydrogen phosphate solution into a silver nitrate solution, finally adjusting the pH value to 8 by using ammonia water, stirring, aging, filtering, washing a filter cake to be neutral, then adding n-butyl alcohol, uniformly stirring, naturally drying by distillation at 80 DEG C, and obtaining the high-surface-area Ag / Ca3 (PO4) 2 catalyst with the hydrophobic surface. The preparation method comprises the following steps: preparing an Ag / Ca3 (PO4) 2 catalyst, drying at 120 DEG C to obtain a precursor, roasting and grinding the precursor at 550 DEG C to obtain a primary product of the Ag / Ca3 (PO4) 2 catalyst, adding deionized water and tetraethoxysilane, reacting and refluxing, carrying out suction filtration, and drying to obtain the high-surface-area Ag / Ca3 (PO4) 2 catalyst with a hydrophobic surface. The invention also provides application of the catalyst. The catalyst is used for catalyzing oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone. The catalyst prepared by the method disclosed by the invention is applied to a reaction for synthesizing methoxyacetone by oxidative dehydrogenation of 1-methoxy-2-propanol, and has high conversion rate and high selectivity performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a method for preparing a high-surface-area Ag / Ca3(PO4)2 catalyst having a hydrophobic surface and an application of the catalyst in catalyzing highly selective oxidative dehydrogenation of alcohol compounds to synthesize ketone compounds. Background Art

[0002] Methoxyacetone (MOA) is a key fine chemical product in the chemical production process, with the two advantages of low toxicity and high efficiency. It is mainly used as an intermediate in the production of pre-emergence herbicide - isopropylamine. There are many methods for synthesizing methoxyacetone. It can be prepared by hydrolysis of formate under the action of acid catalyst and then purified by distillation; it can also be synthesized under suitable conditions by condensation reaction of acetone and methanol. In addition to the above methods, the dehydrogenation of methoxypropanol (MOP) to synthesize methoxyacetone is currently the most important preparation route. However, due to the thermodynamic equilibrium limitation of the direct dehydrogenation process, the conversion rate of methoxypropanol is not high. The use of oxidative dehydrogenation process can break the thermodynamic equilibrium limitation, obtain a higher MOP conversion rate, and even completely convert it. However, since oxidative dehydrogenation generates water, it will cause side reactions such as hydrolysis reaction and cracking reaction, resulting in low selectivity of the target product methoxyacetone.

[0003] In 1949, Raymond PM et al. used sodium dichromate-sulfuric acid chemical oxidation to prepare MOA. Although the conversion rate was quite high, the product selectivity was extremely poor and the environmental pollution was serious. In contrast, the Pd / C catalyst catalytic oxidation method can obtain products with higher selectivity, but the catalyst is easily poisoned and deactivated. A study in 1996 found that the selectivity of the special titanium-silicon system was also high, but the reaction time was long and the catalyst dosage was large. Although the sodium tungstate-hydrogen peroxide acidic system can effectively convert MOP, it also faces this problem; subsequent studies have effectively promoted the oxidation of methoxypropanol by adding additives such as methanol and acetonitrile, thereby increasing the yield of methoxyacetone. In metal heterogeneous catalytic systems, Cu-based catalysts have attracted widespread attention due to their abundant resources, low cost and good catalytic performance, but the life of the Cu-NiPO4 catalyst is only 2 hours, and although the commercial Cu-Zn / Al2O3 catalyst has good stability, the raw material conversion rate is only 50.3%. In 2002, Wang Junwei et al. developed a highly active Cu-Ni / SiO2 catalyst in the synthesis of MOA, but the activity of the catalyst could only be maintained for 8 hours at high temperature. In recent years, copper-based catalysts prepared by co-precipitation have been popular. Zhao et al. prepared a Cu-Al2O3 catalyst by using an improved co-precipitation method. The catalyst exhibited high specific surface area and high dispersion, which enabled the conversion rate of the raw material to reach more than 80%. However, its selectivity was only about 50%. In order to further improve the performance, they introduced silicon and prepared a catalyst with Cu loaded on a SiO2-Al2O3 composite carrier. This strategy effectively suppressed the acid content of the catalyst, resulting in an increase in the conversion rate of MOP to 95.8%, while the selectivity of MOA also reached 75.8%.

[0004] Silver-based catalysts have good chemical stability. At the same time, since silver catalysts have moderate oxygen adsorption properties (copper catalysts have oxygen affinity, and gold catalysts have anaerobic properties), they are conducive to the oxidative dehydrogenation reaction of methoxypropanol. However, it still has strong acidity, resulting in low selectivity for methoxyacetone. If conventional alkaline carriers such as magnesium oxide are used to adjust the acidity and alkalinity of the catalyst surface, magnesium oxide has strong alkalinity and can still catalyze the hydrolysis reaction, resulting in unsatisfactory selectivity for methoxyacetone.

[0005] The existing catalysts for the oxidative dehydrogenation reaction of methoxypropanol have problems such as low methoxypropanol conversion rate, low methoxyacetone selectivity, and short catalyst life. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface and its application in view of the deficiencies of the above-mentioned prior art. The catalyst is used in the reaction of oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone, and has high conversion rate and high selectivity performance.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface, the method comprising:

[0008] S1. Add distilled water to calcium nitrate tetrahydrate to dissolve it, so as to obtain a calcium nitrate solution;

[0009] Add distilled water to diammonium hydrogen phosphate to dissolve it, so as to obtain diammonium hydrogen phosphate solution;

[0010] Add the calcium nitrate solution and diammonium hydrogen phosphate solution dropwise to the silver nitrate solution, and finally adjust the pH value to 8 with aqueous ammonia to obtain a solution to be treated;

[0011] S2, stirring the solution to be treated obtained in S1 at 90° C. for 5 h, aging at room temperature for 24 h, filtering, and washing the filter cake to neutrality to obtain a washed primary product;

[0012] S3, adding n-butanol to the washed primary product obtained in S2, stirring evenly, evaporating naturally at a temperature of 80° C., and then continuing to dry the solid at a temperature of 120° C. for 12 hours to obtain a precursor;

[0013] S4, heating the precursor obtained in S3 from room temperature to 550°C at a heating rate of 5°C / min, maintaining the constant temperature for 5h, then naturally cooling to room temperature, and grinding to obtain a preliminary product of Ag / Ca3(PO4)2 catalyst;

[0014] S5. Add deionized water to the initial Ag / Ca3(PO4)2 catalyst obtained in S4, stir, add tetraethoxysilane, reflux at 100°C for 2h, cool naturally to room temperature, filter, and dry to obtain a high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface. (The words "stir fully" and "stir fully" cannot be used in the claims, but can be placed in the specification)

[0015] Preferably, the mass ratio of the calcium nitrate tetrahydrate, diammonium hydrogen phosphate and silver nitrate in the silver nitrate solution in S1 is 7.08 g:2.64 g:0.34 g.

[0016] Preferably, the washing method in S2 is: firstly, washing by suction with deionized water twice, and then washing by suction with anhydrous ethanol twice.

[0017] Preferably, the high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface in S5 has a specific surface area of ​​120 m 2 / g~150m 2 / g.

[0018] Preferably, the amount of tetraethoxysilane used in S5 is 2% to 4% of the initial mass of the Ag / Ca3(PO4)2 catalyst.

[0019] The present invention also provides the use of a high surface area Ag / Ca3(PO4)2 catalyst having a hydrophobic surface prepared by the above preparation method, wherein the high surface area Ag / Ca3(PO4)2 catalyst having a hydrophobic surface is used to catalyze the oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] The catalyst preparation conditions of the present invention are mild, the process cost is low, and the catalyst is prepared by a coprecipitation method of drying with n-butanol, which can significantly increase the specific surface area of ​​the catalyst and the dispersion of silver ions, thereby improving the catalytic activity. Silver has high chemical stability and high catalytic activity for oxidation reactions. Calcium phosphate has weak alkalinity or partial neutrality. When silver ions are added, the acidity and alkalinity are mutually neutralized, thereby reducing the catalytic effect of hydrolysis reaction and cracking reaction, and improving the selectivity of methoxyacetone. The outside of the catalyst has a hydrophobic coating of tetraethoxysilane, which can prevent the generated water from contacting the active sites on the catalyst surface, thereby reducing the catalytic effect of hydrolysis reaction and improving the selectivity of methoxyacetone. The catalyst of the present invention is used in the catalytic reaction of synthesizing methoxyacetone by oxidative dehydrogenation of 1-methoxy-2-propanol, and has high conversion rate and high selectivity performance.

[0022] The present invention is further described in detail below in conjunction with embodiments. DETAILED DESCRIPTION

[0023] Example 1

[0024] The preparation method of the high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface of this embodiment is as follows:

[0025] S1. Add 100 mL of distilled water to 7.08 g of calcium nitrate tetrahydrate to dissolve the mixture to obtain a calcium nitrate solution;

[0026] Add 100 mL of distilled water to 2.64 g of diammonium hydrogen phosphate to dissolve it to obtain a diammonium hydrogen phosphate solution;

[0027] Add the calcium nitrate solution and diammonium hydrogen phosphate solution dropwise to 400 mL of silver nitrate aqueous solution (containing 0.34 g of silver nitrate) at 90° C., and finally adjust the pH value to 8 with ammonia water to obtain a solution to be treated;

[0028] S2, stirring the liquid to be treated obtained in S1 at a temperature of 90° C. for 5 h, aging at room temperature for 24 h, filtering, and washing the filter cake twice with deionized water, and then washing twice with anhydrous ethanol until neutral, to obtain a washed primary product;

[0029] S3, adding n-butanol to the washed primary product obtained in S2, stirring evenly, evaporating naturally at a temperature of 80° C., and then continuing to dry the solid at a temperature of 120° C. for 12 hours to obtain a precursor;

[0030] S4. The precursor obtained in S3 is placed in a muffle furnace, and the temperature is increased from room temperature to 550°C at a heating rate of 5°C / min, and the temperature is maintained constant for 5 hours, and then naturally cooled to room temperature. After grinding, the initial Ag / Ca3(PO4)2 catalyst is obtained.

[0031] In this embodiment, the raw material calcium phosphate is used as a carrier, which has a weak alkalinity or is slightly neutral. The addition of silver ions can basically neutralize the acidity and alkalinity, thereby reducing the catalytic effect of the hydrolysis reaction and improving the selectivity of methoxyacetone;

[0032] The co-precipitation method improved by drying with n-butanol can significantly increase the specific surface area of ​​the catalyst and the dispersion of silver ions, thereby improving the catalytic activity;

[0033] S5, add 60mL of deionized water to 3g of the initial Ag / Ca3(PO4)2 catalyst obtained in S4, stir thoroughly at room temperature, add 0.06g of tetraethoxysilane, reflux at 100°C for 2h, cool naturally to room temperature, filter and dry to obtain a catalyst with a specific surface area of ​​120m 2 / g of high surface area Ag / Ca3(PO4)2 catalyst with hydrophobic surface.

[0034] In this embodiment, a hydrophobic coating is applied to the outer surface of the Ag / Ca3(PO4)2 catalyst prepared in S3, so that the generated water does not contact the active sites on the catalyst surface, thereby reducing the catalytic effect of the hydrolysis reaction and improving the selectivity of methoxyacetone.

[0035] The high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface prepared in this example was used to catalyze the oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone.

[0036] Catalytic reaction: A micro digital fixed bed reactor (YZBPR-G3L1-2X, Shanghai Yanzheng Experimental Instrument Co., Ltd.) was used to carry out the catalytic oxidation experiment of 1-methoxy-2-propanol. The composition and content of the product were analyzed by gas chromatography to evaluate the catalytic performance of the catalyst.

[0037] (1) The raw material MOP is fed into the reactor through a micro-feed pump.

[0038] (2) Weigh 1 g of catalyst (the high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface prepared in this example). First, lay a thin layer of quartz wool in the reaction tube, then fill in quartz sand, catalyst, and quartz sand in order, and finally fill the outside of the quartz sand with an appropriate amount of quartz wool.

[0039] (3) Install the reaction tube containing the catalyst and let air in to check whether the tube is leaking.

[0040] (4) After confirming that there is no leakage, set the preheating temperature to 200°C and the reaction temperature to 300°C, then start the heating program and heat it to the preset value at a rate of 10°C / min.

[0041] (5) Set the air volume flow rate to 80 mL / min and adjust the liquid hourly space velocity (1.8 mL g -1 ·h -1 )Pump the raw material MOP into the system through a pump.

[0042] (6) The raw materials are vaporized and reacted in the catalyst bed. The generated gas phase products are condensed and collected in the product storage tank.

[0043] (7) Take samples at regular intervals. Drain all remaining liquid in the tank 5 minutes before taking samples. This is to eliminate the impact of any residue in the pipeline on the experimental results.

[0044] (8) When the reaction is complete, first stop the feed pump of the raw material, then turn off the heating program. Next, continue to let air in for a while to clean the residual liquid in the pipeline. After the system cools down to room temperature, turn off the reactor.

[0045] The conversion rate of raw material MOP is 98.56%, the selectivity of target product MOA is 98.67%, and the reaction is stable for 150 hours. The reaction result is far superior to the performance of traditional catalysts such as Ag / SiO2, Ag / MgO-SiO2, Cu-Zn / Al2O3, etc. This is mainly due to the method of the present invention: (1) The high surface area silver / calcium phosphate is prepared by an improved coprecipitation method. The method can obtain a silver / calcium phosphate catalyst with a high surface area and high dispersion, thereby improving the catalytic activity. (2) Calcium phosphate is used as a carrier, which has weak alkalinity or partial neutrality. The addition of silver can basically neutralize the acid and alkalinity by mixing in a suitable proportion, thereby reducing the side reactions such as cracking reaction and hydrolysis reaction under acid and base catalysis, and improving the selectivity of methoxyacetone. (3) The catalyst is coated with a hydrophobic coating, which can prevent the water generated by oxidative dehydrogenation from contacting the active site on the catalyst surface, thereby reducing the catalytic effect of the hydrolysis reaction and improving the selectivity of methoxyacetone.

[0046] Example 2

[0047] The preparation method of the high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface of this embodiment is as follows:

[0048] S1. Add 100 mL of distilled water to 7.08 g of calcium nitrate tetrahydrate to dissolve the mixture to obtain a calcium nitrate solution;

[0049] Add 100 mL of distilled water to 2.64 g of diammonium hydrogen phosphate to dissolve it to obtain a diammonium hydrogen phosphate solution;

[0050] Add the calcium nitrate solution and diammonium hydrogen phosphate solution dropwise to 400 mL of silver nitrate aqueous solution (containing 0.34 g of silver nitrate) at 90° C., and finally adjust the pH value to 8 with ammonia water to obtain a solution to be treated;

[0051] S2, stirring the liquid to be treated obtained in S1 at a temperature of 90° C. for 5 h, aging at room temperature for 24 h, filtering, and washing the filter cake twice with deionized water, and then washing twice with anhydrous ethanol until neutral, to obtain a washed primary product;

[0052] S3, adding n-butanol to the washed primary product obtained in S2, stirring evenly, evaporating naturally at a temperature of 80° C., and then continuing to dry the solid at a temperature of 120° C. for 12 hours to obtain a precursor;

[0053] S4. The precursor obtained in S3 is placed in a muffle furnace, and the temperature is increased from room temperature to 550°C at a heating rate of 5°C / min, and the temperature is maintained constant for 5 hours, and then naturally cooled to room temperature. After grinding, the initial Ag / Ca3(PO4)2 catalyst is obtained.

[0054] In this embodiment, the raw material calcium phosphate is used as a carrier, which has a weak alkalinity or is slightly neutral. The addition of silver ions can basically neutralize the acidity and alkalinity, thereby reducing the catalytic effect of the hydrolysis reaction and improving the selectivity of methoxyacetone;

[0055] The co-precipitation method improved by drying with n-butanol can significantly increase the specific surface area of ​​the catalyst and the dispersion of silver ions, thereby improving the catalytic activity;

[0056] S5, add 60mL of deionized water to 3g of the initial Ag / Ca3(PO4)2 catalyst obtained in S4, stir thoroughly at room temperature, add 0.12g of tetraethoxysilane, reflux at 100°C for 2h, cool naturally to room temperature, filter and dry to obtain a catalyst with a specific surface area of ​​150m 2 / g of high surface area Ag / Ca3(PO4)2 catalyst with hydrophobic surface.

[0057] The high surface area Ag / Ca3(PO4)2 catalyst with a hydrophobic surface prepared in this example was used to catalyze the oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone.

[0058] The catalytic reaction method is the same as in Example 1.

[0059] The conversion rate of raw material MOP was 98.76%, the selectivity of target product MOA was 98.85%, and it ran stably for 150 hours.

[0060] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high surface area Ag / Ca with a hydrophobic surface 3 (PO 4 ) 2 A method for preparing a catalyst, It is characterized in that The method is: S1. Add distilled water to calcium nitrate tetrahydrate to dissolve it, so as to obtain a calcium nitrate solution; Add distilled water to diammonium hydrogen phosphate to dissolve it, so as to obtain diammonium hydrogen phosphate solution; Add the calcium nitrate solution and diammonium hydrogen phosphate solution dropwise to the silver nitrate solution, and finally adjust the pH value to 8 with aqueous ammonia to obtain a solution to be treated; S2, stirring the solution to be treated obtained in S1 at 90° C. for 5 h, aging at room temperature for 24 h, filtering, and washing the filter cake to neutrality to obtain a washed primary product; S3, adding n-butanol to the washed primary product obtained in S2, stirring evenly, evaporating naturally at a temperature of 80° C., and then continuing to dry the solid at a temperature of 120° C. for 12 hours to obtain a precursor; S4, the precursor obtained in S3 was heated from room temperature to 550°C at a heating rate of 5°C / min, kept at a constant temperature for 5h, then naturally cooled to room temperature, and ground to obtain Ag / Ca 3 (PO 4 ) 2 Catalyst initial product; S5, Ag / Ca obtained from S4 3 (PO 4 ) 2 Deionized water was added to the catalyst, and after stirring, tetraethoxysilane was added. The mixture was refluxed at 100°C for 2 h, and then naturally cooled to room temperature, filtered, and dried to obtain a high surface area Ag / Ca catalyst with a hydrophobic surface. 3 (PO 4 ) 2 catalyst.

2. A high surface area Ag / Ca with a hydrophobic surface according to claim 1. 3 (PO 4 ) 2 A method for preparing a catalyst, It is characterized in that The mass ratio of the calcium nitrate tetrahydrate, diammonium hydrogen phosphate and silver nitrate in the silver nitrate solution in S1 is 7.08 g:2.64 g:0.34 g.

3. A high surface area Ag / Ca with a hydrophobic surface according to claim 1. 3 (PO 4 ) 2 A method for preparing a catalyst, It is characterized in that The washing method in S2 is: first, filter and wash twice with deionized water, and then filter and wash twice with anhydrous ethanol.

4. A high surface area Ag / Ca with a hydrophobic surface according to claim 1. 3 (PO 4 ) 2 A method for preparing a catalyst, It is characterized in that High surface area Ag / Ca with hydrophobic surface as described in S5 3 (PO 4 ) 2 The specific surface area of ​​the catalyst is 120m 2 / g~150m 2 / g.

5. A high surface area Ag / Ca with a hydrophobic surface according to claim 1. 3 (PO 4 ) 2 A method for preparing a catalyst, It is characterized in that The amount of tetraethoxysilane used in S5 is Ag / Ca 3 (PO 4 ) 2 2% to 4% of the initial quality of the catalyst.

6. A high surface area Ag / Ca with a hydrophobic surface prepared by the method of any one of claims 1 to 5 3 (PO 4 ) 2 Application of catalysts, It is characterized in that The high surface area Ag / Ca 3 (PO 4 ) 2 The catalyst is used for catalyzing the oxidative dehydrogenation of 1-methoxy-2-propanol to synthesize methoxyacetone.