Method for preparing porous zeolite composite material from iron tailings and application of porous zeolite composite material
Through alkali melt-hydrothermal method, fine-grained iron tailings were recombined, and porous zeolite composite materials with excellent catalytic oxidation performance were prepared, which solved the problem of resource utilization of iron tailings fine powder, achieved efficient removal of antibiotic pollutants, and promoted the promotion of Wastewater purification.
Patent Information
- Application Number
- CN202411464338.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-21
AI Technical Summary
The prior art is difficult to effectively utilize iron tailings fine powder with a particle size of less than 0.075 mm, and its chemical composition is uneven and its mineral structure is low, resulting in high cost of preparation of zeolite materials and poor product controllability, and failure to achieve porous zeolite composites. Efficient resource utilization of materials.
The alkali melt-hydrothermal method is used to recombinate the fine-grained iron tailings mineral structure to synthesize the porous zeolite composite material in the micron-scale octahedral form, and realize its in-situ doping of Fe elements and surface loading. Catalytic oxidation performance, efficient removal of emerging pollutants such as antibiotics.
The prepared porous zeolite composite material has uniform particle size, rich pores, high specific surface area and excellent catalytic oxidation properties, which significantly improves the removal efficiency of antibiotic pollutants, promotes the resource utilization and high-value utilization of iron tailings, and solves the problem of Wastewater purification problem.
Smart Images

Figure CN119056484A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing environmental functional materials from industrial solid waste and high-value utilization, and specifically relates to a method for preparing a porous zeolite composite material from iron tailings and use thereof. Background Art
[0002] Iron tailings are solid wastes generated during the process of crushing, grinding and beneficiation of iron ore to obtain iron concentrate. Due to the low grade of iron ore in my country, the beneficiation process needs to go through two or even three stages of grinding, resulting in finer iron tailings. The fine iron tailings with a particle size of less than 0.075 mm account for more than 30% of the total tailings, posing a serious threat to regional air quality, water quality and environmental safety. At present, coarser iron tailings can be widely used in the building materials industry as sand and gravel aggregates, cement clinker and cementitious materials, while the resource-efficient utilization of fine iron tailings with a particle size of less than 0.075 mm has become an environmental and resource problem that needs to be solved urgently. Generally speaking, iron tailings powder contains a small amount of iron minerals and rich silicon and aluminum components. The mineral composition is mainly silicate minerals such as quartz, feldspar and mica, showing the characteristics of low monomer dissociation, stable mineral structure and low chemical activity. By regulating the basic structural units of iron tailings minerals and reconstructing the mineral phase, fine-grained iron tailings can be converted into high-value-added mineral functional materials such as mesoporous silicates, mesoporous silica, zeolite molecular sieves, etc., which can be used to solve ecological and environmental problems and mineral resource shortages.
[0003] Zeolite is a crystalline three-dimensional porous aluminosilicate. [SiO4] and [AlO4] tetrahedral units are connected by oxygen atoms to construct a multi-porous cage structure, so that the zeolite framework can accommodate water molecules, potassium, sodium, calcium ions and small organic molecules, thereby showing excellent adsorption, catalytic and ion exchange properties. At present, there have been many studies on the use of industrial solid wastes such as coal gangue, fly ash and red mud as cheap raw materials to synthesize zeolite materials. However, there are fewer studies on the preparation of zeolite materials from iron tailings as raw materials. This is because the chemical composition of iron tailings is uneven, the mineral phase structure is stable, and the reaction activity is low, which makes the synthesis of zeolite from iron tailings have high process costs and poor product controllability. For example, CN117105241A discloses an ionic rare earth tailings-based zeolite material and a method for removing lead ions from a solution. The thermally activated tailings are reacted with a NaOH solution in an oil bath to form a cubic A-type zeolite, which has a strong acidic effect on Pb 2+It showed good adsorption effect, with an adsorption amount of up to 53.91 mg / g, proving the practical application potential of zeolite materials synthesized from tailings in the field of removing water pollutants. However, there has been no report on the in-situ conversion of multi-components such as Si, Al, and Fe in iron tailings into metal-loaded porous zeolite composites, combined with the pore structure and surface adsorption characteristics of zeolite, and the coordinated in-situ loaded transition metal Fe element to achieve pollutant enrichment and advanced oxidation degradation, and applied to the removal of organic pollutants in wastewater.
[0004] Therefore, in view of the problems and shortcomings of the existing preparation of zeolite materials from iron tailings, the present invention proposes a method for preparing fine-grained iron tailings with complex components and low reaction activity through a simple alkali melting-hydrothermal process, which has uniform particle size, rich pores, high specific surface area and excellent catalytic oxidation performance. The porous zeolite composite material can catalyze the degradation of emerging pollutants such as antibiotics, promote the efficient and high-value utilization of solid waste resources, and promote the solution to the problem of wastewater purification. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the first aspect of the present invention is to provide a method and use for preparing a porous zeolite composite material from iron tailings. The present invention adopts an alkali melting-hydrothermal method to reorganize the mineral structure of fine-grained iron tailings, synthesize a porous zeolite composite material in the form of a micron-sized octahedron, and simultaneously realizes the in-situ doping and surface loading of the Fe element, so that it exhibits excellent catalytic oxidation performance in a Fenton-like system, can efficiently remove emerging pollutants such as antibiotics, and realize the resource and high-value utilization of all components of iron tailings. The purpose of the second aspect is to provide a method for preparing a FAU-type porous zeolite composite material from iron tailings.
[0006] In order to achieve the above technical purpose, the technical solution of the present invention is: In a first aspect, the present invention provides a method for preparing a porous zeolite composite material from iron tailings, wherein fine iron tailings and Al2O3 powder are activated by alkali melting to obtain an alkali-activated raw material; the alkali-activated raw material is then mixed with water at a liquid-to-solid ratio of 5:1-9:1, and a hydrothermal crystallization reaction is performed at 90-120°C to obtain a porous zeolite composite material; The particle size of the fine iron tailings is not greater than 0.075 mm, the mass content of SiO2 is not less than 60%, and the mass content of Fe2O3 is not less than 6%; the molar ratio of SiO2 to Al2O3 is adjusted to 2.0-5.5 by adding Al2O3 powder.
[0007] Preferably, the molar ratio of SiO2 to Al2O3 is adjusted to 2.7-4.7 by adding Al2O3 powder; the mass content of Fe2O3 in the fine iron tailings is 8-10%; and the mass content of SiO2 is 65-75%.
[0008] Preferably, during alkali fusion activation, inorganic alkali powder is added, the inorganic alkali is at least one of NaOH, KOH, Na2CO3, K2CO3, etc., and the mass ratio of the inorganic alkali powder to the sum of fine iron tailings and Al2O3 powder is 0.8-1.2.
[0009] Preferably, the calcination temperature of the alkali fusion activation is 550-850° C., and the calcination time is 2-4 hours.
[0010] In a second aspect, the present invention protects a porous zeolite composite material obtained by the method, wherein the porous zeolite composite material consists of zeolite and amorphous matter, and the mass content of the FAU type zeolite phase is greater than 10%.
[0011] Preferably, during the synthesis of the porous zeolite composite material, part of Fe replaces Al in the zeolite and enters the framework structure, and part of Fe is solid-dissolved in the amorphous aluminosilicate phase, so that it has higher reactivity and exhibits excellent catalytic oxidation performance for antibiotic pollutants in a Fenton-like system.
[0012] In a third aspect, the present invention provides a method for preparing a FAU-type porous zeolite composite material from iron tailings, wherein fine iron tailings and Al2O3 powder are mixed to obtain a mixed material, wherein the particle size of the fine iron tailings is not greater than 0.075 mm, the mass content of SiO2 is not less than 60%, and the mass content of Fe2O3 is not less than 6%; the molar ratio of SiO2 to Al2O3 is adjusted to 3.7 by adding Al2O3 powder; The mixture was heated to 550 °C in a muffle furnace at a temperature program of 5 °C / min and calcined for 3 h, and then cooled to obtain an alkali-activated raw material; The alkali-activated raw material was then mixed evenly with water at a liquid-to-solid ratio of 5:1, and then hydrothermally crystallized at 100 °C for 14 h to obtain a FAU-type porous zeolite composite material.
[0013] Preferably, the FAU-type porous zeolite composite material comprises a FAU-type faujasite zeolite with a complete structure and regular morphology and a surface-loaded amorphous aluminosilicate, and has a composite pore structure with abundant micropores and partial mesopores, an average pore diameter of 1.94 nm, and a total pore volume of 0.259 cm 3 / g, with a specific surface area of 534.06 m 2 / g.
[0014] In a fourth aspect, the present invention provides an application of a material prepared by the above method, wherein the porous zeolite composite material is used for catalytic degradation of organic pollutants in wastewater.
[0015] For the degradation of tetracycline hydrochloride, a tetracycline hydrochloride solution with an initial concentration of no more than 400 mg / L is prepared in a conical flask, the initial pH of the solution is adjusted to 2-3, 0.2-1.0 g / L of the porous zeolite composite material is added to the tetracycline hydrochloride solution, and after adding 10 mM H2O2 solution, it is placed in an oscillating box for reaction, and a degradation rate of more than 90% is achieved within 20-120 minutes.
[0016] More preferably, the initial concentration of the tetracycline hydrochloride solution is 10-200 mg / L; the initial pH of the solution is adjusted to 2; and the amount of the porous zeolite composite material added is 0.4 g / L.
[0017] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses alkali fusion activation-hydrothermal crystallization to synthesize FAU-type porous zeolite composite materials from iron tailings. In the alkali fusion activation process, inert mineral components such as quartz are converted into soluble silicates and aluminates, and the dissolution of metal elements in the tailings is promoted. In the subsequent hydrothermal crystallization process, structural units such as Si and Al are reorganized into a porous zeolite composite material in the form of micron-sized octahedrons.
[0018] (2) The present invention uses unremoved fine iron tailings as raw materials, retains impurity elements mainly composed of iron, and realizes efficient resource utilization of multiple components such as Si, Al and Fe. During the structural reconstruction process, some highly active Fe ions replace part of the Al in the zeolite framework to achieve in-situ doping, while the other part of Fe is solid-dissolved in amorphous aluminosilicate nanoparticles and deposited on the surface of the zeolite material.
[0019] (3) The porous zeolite composite material prepared by the present invention has the characteristics of high specific surface area, uniform particle size and controllable structural composition. The in-situ doping and surface loading of Fe element make it have excellent catalytic oxidation performance. As a Fenton catalytic material, it shows excellent potential in wastewater treatment and provides ideas for the utilization of all components of iron tailings. Through experimental tests, in a Fenton-like system, the porous zeolite composite material prepared from iron tailings has a significant removal effect on antibiotic pollutants and is significantly better than natural zeolite and pure silicon-aluminum source synthetic zeolite.
[0020] The present application uses the components of tailings waste to participate in the entire crystallization step, and does not require the addition of additional metal reagents. The iron tailings are directly synthesized into a zeolite composite material without impurity removal. The material has zeolite characteristics and exhibits excellent catalytic oxidation performance due to the in-situ loading of Fe. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD patterns of the porous zeolite composite materials prepared in Examples 1-8 and the materials prepared in Comparative Examples 1 and 2; Figure 2 This is a SEM image of the porous zeolite composite material prepared in Example 6; Figure 3 N2 adsorption-desorption curve and pore size distribution diagram of the porous zeolite composite material prepared in Example 6; Figure 4 This is an XPS graph of the porous zeolite composite material prepared in Example 6; Figure 5 A comparison chart of the adsorption and catalytic degradation of tetracycline hydrochloride by the materials prepared in Example 6 and Comparative Examples 1 and 2; Figure 6 This is the catalytic degradation curve of the porous zeolite composite material prepared in Example 6 to tetracycline hydrochloride with different initial concentrations. DETAILED DESCRIPTION
[0022] In order to more clearly describe the purpose, technical solutions and advantages of the present invention, the following examples are combined to further illustrate the content of the invention, rather than to limit the protection scope of the present invention.
[0023] The method for preparing a porous zeolite composite material from iron tailings of the present invention comprises the following steps: (1) Alkali fusion activation: fine iron tailings and Al2O3 powder are activated by alkali fusion to obtain alkali-activated raw materials; Al2O3 powder is used to adjust the silicon-aluminum ratio. Inorganic alkali powder needs to be added during alkali fusion activation. Alkali fusion activation enables fine iron tailings and Al2O3 powder to be completely alkali-fused at high temperature.
[0024] The particle size of the fine iron tailings is not greater than 0.075 mm, the SiO2 content is not less than 60%, and the Fe2O3 content is not less than 6%. The molar ratio of SiO2 to Al2O3 in the mixture of fine iron tailings and Al2O3 powder is 2.0-5.5, preferably 2.7-4.7. When the molar ratio of SiO2 to Al2O3 is too small, such as 1.0, the composite material is prone to form a mixed phase and has poor stability. When the molar ratio of SiO2 to Al2O3 is too large, it is easy to have the problem of difficulty in crystallization.
[0025] (2) Hydrothermal crystallization: Add water to the alkali-activated raw material and stir it at a liquid-to-solid ratio of 5:1-9:1 to obtain a precursor suspension, which is then poured into a polytetrafluoroethylene-lined reactor for hydrothermal crystallization at a temperature of 90-120 °C. The crystallized product is filtered, washed, and dried to obtain a porous zeolite composite material.
[0026] As a preferred solution, the inorganic base used in step (1) is at least one of NaOH, KOH, etc., and the mass ratio of the inorganic base powder to the mixed powder (the sum of the fine iron tailings and Al2O3 powder) is 0.8-1.2.
[0027] As a preferred solution, in step (1), the calcination temperature is 550-850°C and the holding time is 2-4 h.
[0028] As a preferred solution, in step (2), the hydrothermal crystallization temperature is 90-110°C and the time is 14 h.
[0029] In the present invention, tetracycline hydrochloride is selected as a representative pollutant to test the catalytic oxidation performance of the material, and the specific steps are as follows: 50 mL of tetracycline hydrochloride solution with an initial concentration of 200 mg / L is prepared in a conical flask, the initial pH of the solution is adjusted to 2, 0.4 g / L of the porous zeolite composite material is added to the tetracycline hydrochloride solution, 10 mM H2O2 solution is added, and the mixture is placed in an oscillating box for reaction. After reacting for 3 h, 3 mL of the supernatant is filtered through a 0.45 μm filter membrane, and the absorbance of the filtrate is measured at a wavelength of 355 nm using an ultraviolet-visible spectrophotometer, and the degradation efficiency of the tetracycline hydrochloride pollutant is calculated based on the measured absorbance value and the standard curve.
[0030] In the following embodiments of the present invention, the fine iron tailings raw materials were ground (passed through a 200-mesh sieve) and dried, and the chemical composition of the iron tailings was measured by X-ray fluorescence spectrometer (XRF) as shown in Table 1.
[0031]
[0032] Example 1 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio (mass ratio of inorganic alkali powder to the sum of fine iron tailings and Al2O3 powder) to 1.0 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for calcination for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 7:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0033] By attaching Figure 1 The XRD pattern shown in the figure shows that the porous zeolite composite material prepared in this example is mainly composed of FAU zeolite, with a certain amount of A zeolite, and other miscellaneous peaks with complex peak shapes. Using Jade 6.0 software and peak fitting method, the FAU zeolite phase content in the zeolite composite material is about 52.77%, and the specific surface area is 200.93 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 97.51% for tetracycline hydrochloride in aqueous solution.
[0034] Example 2 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.0 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min and calcine it for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 7:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 90 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0035] By attaching Figure 1 The XRD pattern shown in the figure shows that the porous zeolite composite material prepared in this example is mainly composed of quartz and amorphous phases, and the zeolite content is relatively low. Using Jade 6.0 software, the peak fitting method is used to calculate that the FAU zeolite phase content in the zeolite composite material is about 27.73%, and the specific surface area is 36.25 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 96.64% for tetracycline hydrochloride in aqueous solution.
[0036] Example 3 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.0 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min and calcine it for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 7:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 110 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0037] By attaching Figure 1 The XRD pattern shows that the porous zeolite composite material prepared in this example is mainly composed of FAU zeolite, and also contains a certain amount of A-type zeolite and P-type zeolite. Using Jade 6.0 software and peak fitting method, the content of FAU zeolite in the zeolite composite material is about 52.37%, and the specific surface area is 200.09 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 97.66% for tetracycline hydrochloride in aqueous solution.
[0038] Example 4 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 2.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.0 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for calcination for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 7:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0039] By attaching Figure 1 The XRD diagram shows that the porous zeolite composite material prepared in this example is mainly composed of type A zeolite, with a lower content of FAU zeolite and a small amount of quartz. Using Jade 6.0 software and peak fitting method, the content of FAU zeolite phase in the zeolite composite material is about 22.99%, and the specific surface area is 112.34 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 96.83% for tetracycline hydrochloride in aqueous solution.
[0040] Example 5 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 4.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.0 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 7:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0041] By attaching Figure 1 The XRD pattern shown in the figure shows that the porous zeolite composite material prepared in this example has a large amount of amorphous phase, the formed FAU type zeolite phase content is small, and there are more miscellaneous peaks. Using Jade 6.0 software, the peak fitting method was used to calculate that the FAU type zeolite phase content in the zeolite composite material was about 30.14%, and the specific surface area was 130.40 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 97.34% for tetracycline hydrochloride in aqueous solution.
[0042] Example 6 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.2 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for calcination for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 5:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0043] Attached Figure 1 The XRD pattern of Example 6 shows that a single type of FAU zeolite phase is synthesized, with sharp peaks and no other impurity peaks. The FAU zeolite phase content is calculated to be 83.43% by the peak fitting method using Jade 6.0 software. Figure 2 It can be clearly seen from the SEM image that the spherical zeolite particles with a particle size of about 2 μm are evenly distributed and well grown, and the flocculent material on the surface of the grains is amorphous aluminosilicate particles; the EDS spectrum shows that the O, Si, Al and Fe elements are evenly distributed, confirming the in-situ doping of Fe in the framework structure and the surface loading of the zeolite material. Figure 3 The N2 adsorption-desorption curve and pore size distribution diagram show that the prepared porous zeolite material has abundant microporous structure and a small amount of mesoporous structure, and its specific surface area is 534.10 m 2 / g, the average pore diameter is 1.94 nm, and the total pore volume is 0.259 cm 3 / g. Attached Figure 4 The XPS spectrum further confirmed the uniform distribution of iron in the material, and the main 3+ The tetracycline hydrochloride removal performance test results show that the catalytic degradation rate of the material for tetracycline hydrochloride in aqueous solution is 97.51%.
[0044] Example 7 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio to 1.2 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for calcination for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 9:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0045] By attaching Figure 1The XRD diagram shown shows that the porous zeolite composite material prepared in this example contains A-type zeolite, P-type zeolite and FAU-type zeolite phases, but the content of FAU-type zeolite phase is very small. In addition, quartz and a large amount of amorphous aluminosilicate are present, and the peak shape is complex. Using Jade 6.0 software and peak fitting method, the content of FAU-type zeolite phase in the zeolite composite material is about 14.37%, and the specific surface area is 73.08 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 97.34% for tetracycline hydrochloride in aqueous solution.
[0046] Example 8 Add Al2O3 powder and iron tailings powder to mix, adjust the molar ratio of SiO2 to Al2O3 to 3.7, then add NaOH solid particles, adjust the alkali-solid ratio to 0.8 and mix. Then pour the mixture into a crucible, heat it to 550 ℃ in a muffle furnace at a temperature program of 5 ℃ / min for calcination for 3 h, and cool it to obtain an alkali-activated raw material. Put the alkali-activated raw material into water at a liquid-solid ratio of 5:1 and stir it for 3 h to obtain a precursor suspension, then pour it into a polytetrafluoroethylene-lined reactor and hydrothermally crystallize it at a temperature of 100 ℃ for 14 h. The crystallized product is filtered, washed and dried to obtain a porous zeolite composite material.
[0047] By attaching Figure 1 The XRD diagram shows that the porous zeolite composite material prepared in this example is mainly composed of quartz, with a certain amount of FAU zeolite and sodalite. Using Jade 6.0 software and peak fitting method, the FAU zeolite content in the zeolite composite material is about 46.02%, and the specific surface area is 166.81 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 97.41% for tetracycline hydrochloride in aqueous solution.
[0048] Comparative Example 1 Al2O3 powder and SiO2 powder were mixed, and the molar ratio of SiO2 to Al2O3 was adjusted to 3.7. Then NaOH solid particles were added, and the alkali-solid ratio was adjusted to 1.2 before mixing. The mixture was then poured into a crucible, heated to 550 °C in a muffle furnace at a temperature program of 5 °C / min for calcination for 3 h, and cooled to obtain an alkali-activated raw material. The alkali-activated raw material was placed in water at a liquid-solid ratio of 5:1 and stirred for 3 h to obtain a precursor suspension, which was then poured into a polytetrafluoroethylene-lined reactor and hydrothermally crystallized at a temperature of 100 °C for 14 h. The crystallized product was filtered, washed, and dried to obtain a zeolite material synthesized from a pure silicon-aluminum source.
[0049] Attached Figure 1The XRD pattern of Comparative Example 1 shows that a single type of FAU zeolite phase is synthesized from pure silicon and aluminum sources, with clear and sharp peaks. Using Jade 6.0 software, the peak fitting method is used to calculate that the FAU zeolite phase content is about 82.45%, and the specific surface area is 492.70 m 2 / g, the tetracycline hydrochloride removal performance test results showed that the material had a removal rate of 9.01% for tetracycline hydrochloride in aqueous solution.
[0050] Comparative Example 2 The natural clinoptilolite is ball-milled and sieved to obtain the natural clinoptilolite powder.
[0051] Attached Figure 1 The XRD diagram of Comparative Example 2 shows that the phase composition of natural clinoptilolite powder is mainly clinoptilolite, containing a small amount of microcline. The test results of tetracycline hydrochloride removal performance show that the removal rate of tetracycline hydrochloride in aqueous solution by the natural clinoptilolite is 18.29%.
[0052] Attached Figure 5 The experiment was carried out under the condition of a pollutant concentration of 50 mg / L. The results showed that the FAU zeolite prepared by pure silicon-aluminum source in Comparative Example 1 and the natural clinoptilolite material selected in Comparative Example 2 had a certain adsorption effect on tetracycline hydrochloride in aqueous solution, but the narrow pore structure limited its removal efficiency for tetracycline hydrochloride pollutant, and in the Fenton-like system, it did not show catalytic oxidation activity for tetracycline hydrochloride.
[0053] In summary, suitable hydrothermal temperature can promote the formation of FAU zeolite, while higher temperature can easily lead to its transformation into P zeolite. Low silicon-aluminum ratio is easy to form A-type zeolite, but with the increase of silicon-aluminum ratio, the content of FAU zeolite phase increases. In addition, a higher liquid-solid ratio will lead to a decrease in the alkalinity of the system, which is not conducive to the crystallization of zeolite, thereby increasing the phase content of amorphous aluminosilicate; while a lower alkali-solid ratio is difficult to completely activate the inert mineral components in the raw material, which is not conducive to its transformation into zeolite structure.
[0054] Attached Figure 6 The degradation kinetic curve of the porous zeolite composite material prepared in Example 6 for tetracycline hydrochloride solutions with different initial concentrations. At a relatively low initial concentration (10-200 mg / L), the final degradation rate of the porous zeolite composite material for tetracycline hydrochloride can reach more than 95%. When the initial concentration continues to increase to 400 mg / L, the degradation rate in 3 h can still reach 88.19%. This shows that the material has an excellent catalytic oxidation effect on tetracycline hydrochloride pollutants in a Fenton-like system, and the degradation rate is relatively fast.
[0055] Any matters not described in the present invention are applicable to the prior art.
Claims
1. A method for preparing a porous zeolite composite material from iron tailings, characterized in that: The fine iron tailings and Al2O3 powder are activated by alkali melting to obtain an alkali-activated raw material; the alkali-activated raw material is then mixed evenly with water at a liquid-to-solid ratio of 5:1-9:1, and a hydrothermal crystallization reaction is performed at 90-120°C to obtain a porous zeolite composite material; The particle size of the fine iron tailings is not greater than 0.075 mm, the mass content of SiO2 is not less than 60%, and the mass content of Fe2O3 is not less than 6%; the molar ratio of SiO2 to Al2O3 is adjusted to 2.0-5.5 by adding Al2O3 powder.
2. The method according to claim 1, characterized in that: The molar ratio of SiO2 to Al2O3 is adjusted to 2.7-4.7 by adding Al2O3 powder; the mass content of Fe2O3 in the fine iron tailings is 8-10%; and the mass content of SiO2 is 65-75%.
3. The method according to claim 1, characterized in that During alkali fusion activation, inorganic alkali powder is added, wherein the inorganic alkali is at least one of NaOH, KOH, Na2CO3, and K2CO3, and the mass ratio of the inorganic alkali powder to the sum of the fine iron tailings and Al2O3 powder is 0.8-1.
2.
4. The method according to claim 1, characterized in that: The calcination temperature of the alkali fusion activation is 550-850° C., and the calcination time is 2-4 hours.
5. The porous zeolite composite material obtained by the method according to any one of claims 1 to 4, characterized in that: The porous zeolite composite material consists of zeolite and amorphous material, and the mass content of the FAU type zeolite phase is greater than 10%.
6. The porous zeolite composite material according to claim 5, characterized in that: During the synthesis of the porous zeolite composite material, part of Fe replaces Al in the zeolite and enters the framework structure, and part of Fe is solid-dissolved in the amorphous aluminosilicate phase, so that it has higher reaction activity and exhibits excellent catalytic oxidation performance on antibiotic pollutants in a Fenton-like system.
7. A method for preparing a FAU type porous zeolite composite material from iron tailings, characterized in that: The fine iron tailings and Al2O3 powder are mixed to obtain a mixed material, wherein the particle size of the fine iron tailings is not greater than 0.075 mm, the mass content of SiO2 is not less than 60%, and the mass content of Fe2O3 is not less than 6%; the molar ratio of SiO2 to Al2O3 is adjusted to 3.7 by adding Al2O3 powder; The mixture was heated to 550 °C in a muffle furnace at a temperature program of 5 °C / min and calcined for 3 h, and then cooled to obtain an alkali-activated raw material; The alkali-activated raw material was then evenly mixed with water at a liquid-to-solid ratio of 5:1, and then hydrothermally crystallized at 100°C for 14 hours to obtain a FAU-type porous zeolite composite material.
8. The method according to claim 7, characterized in that The FAU-type porous zeolite composite material comprises a FAU-type faujasite zeolite with a complete structure and regular morphology and a surface-loaded amorphous aluminosilicate, and has a composite pore structure with abundant micropores and partial mesopores, an average pore diameter of 1.94 nm, and a total pore volume of 0.259 cm 3 / g, with a specific surface area of 534.06 m 2 / g.
9. Use of the material prepared by the method of any one of claims 1 to 4, 7 and 8, characterized in that: The porous zeolite composite material is used for catalytic degradation of organic pollutants in wastewater; preferably, it is used for the degradation of tetracycline hydrochloride, a tetracycline hydrochloride solution with an initial concentration of no more than 400 mg / L is prepared in a conical flask, the initial pH of the solution is adjusted to 2-3, 0.2-1.0 g / L of the porous zeolite composite material is added to the tetracycline hydrochloride solution, and after adding 10 mM H2O2 solution, it is placed in an oscillation box for reaction, and a degradation rate of more than 90% is achieved within 20-120 minutes.
10. The use according to claim 9, characterized in that: The initial concentration of the tetracycline hydrochloride solution is 10-200 mg / L; the initial pH of the solution is adjusted to 2; and the amount of the porous zeolite composite material added is 0.4 g / L.
Citation Information
Patent Citations
Methodof producing zeolite molecular sieve by utilizing tailings
CN105036151A
Molecular sieve-type Fenton catalyst for elimination of organic dye pollution and high efficiency synthesis method thereof
CN106732747A
Iron-based FAU type zeolite composite material as well as preparation method and application thereof
CN114558545A
Method for preparing analcime from silicon-aluminum tailings
CN115818659A
Preparation and use method of molecular sieve based on iron tailings
CN117776206A