Production method of self-repairing color-coated steel plate for building

By adopting a double-layer coating process on color-coated steel plates, using the self-repair mechanism of nano-container packaging corrosion inhibitor and polyester polyurethane resin, the problems of traditional color steel tiles being easily corroded and coating damage in outdoor environments are solved, and the problem of traditional color steel tiles being easily corroded and damaged in outdoor environments is realized. Efficient self-repair and corrosion resistance, reduce maintenance costs, and are suitable for building materials in complex environments.

CN119056728APending Publication Date: 2024-12-03PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411394577.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional colored steel tiles are prone to corrosion in outdoor environments and easily damaged coatings, resulting in reduced structural strength and safety hazards. The existing self-repair coating cannot be effectively repaired in humid environments, resulting in waste of corrosion inhibitors and high maintenance costs.

Method used

Using the 'coating-drying' two-coating and two-baking continuous production process, a double-layer coating is prepared: self-repair primer layer and weather-resistant topcoat layer, nano-container packaging corrosion inhibitor is added to the primer, and the topcoat layer is made of polyester Polyurethane resin is reformed during damage by non-covalent bonds to repair the damaged site.

Benefits of technology

It realizes self-repair performance in humid environments, extends the service life of color-coated steel plates, reduces maintenance costs, improves the corrosion resistance and decorative properties of the materials, and adapts to applications in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056728A_ABST
    Figure CN119056728A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a self-repairing color-coated steel plate for buildings, which comprises the following steps: carrying out roller coating pretreatment on cleaned coating strip steel, dipping primer and back paint, curing and drying to form a self-repairing primer layer and a back paint layer; the self-repairing primer layer is epoxy resin containing a nanometer container for packaging the corrosion inhibitor, and the addition mass ratio of the nanometer container to the epoxy resin is 0.5%-1%; and dipping the galvanized strip steel coated with the primer in finish paint to form a finish paint layer, and coiling the finish paint layer through an outlet loop. According to the method, the color-coated steel plate with a self-repairing primer and a weather-resistant finish paint is prepared by utilizing a'two-time coating and two-time drying 'process of continuous production of the color-coated steel plate; the color-coated steel plate is environment-friendly, high in corrosion resistance and high in decoration performance, has self-repairability, and can resist erosion of natural factors such as ultraviolet radiation, temperature change and humidity change; the coating can be applied to roofs and wall surfaces of buildings and provides protection and decoration functions for the buildings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a production method of a self-repairing color-coated steel plate for construction. Background Art

[0002] In outdoor environments, traditional color steel tiles made of color-coated sheets for construction are usually exposed to sunlight, rain, moisture, atmospheric pollutants and other conditions for a long time; for example, in some areas with heavy industrial pollution or coastal areas, salt and sulfide in the air will accelerate the corrosion of the surface of color steel tiles. Rainwater may contain acidic substances, which will also corrode the coating and metal substrate of color steel tiles. Extreme weather such as hail and freezing rain will also damage the coating of color steel tiles. As time goes by, rust and coating peeling will occur, thus affecting its service life and appearance. When the coating on the surface of the color steel tile is damaged, the metal substrate is directly exposed to the external environment, and the corrosion rate will be further accelerated, resulting in a gradual decrease in the structural strength of the color steel tile, and there may be safety hazards such as leakage, deformation and even collapse; at the same time, the color steel tile may also be affected by various external forces during installation and use, and the coating will be scratched and damaged due to handling, collision, scratching, etc., causing coating damage.

[0003] For the construction industry, the demand for high-performance, long-life, and low-maintenance building materials is growing. Traditional color steel tiles need to be regularly maintained and replaced due to their shortcomings such as easy corrosion and easy damage to the coating, which not only increases the cost of use, but may also affect the normal use of the building. For example, the patent with publication number CN 101613543B provides a method for preparing a coating with metal surface corrosion inhibition and self-repairing functions, wherein the coating adsorbs polyallyl ammonium chloride in a 1-10% SiO2 / ZrO2 nanoparticle solution to form cationic SiO2 / ZrO2 nanoparticles, which are then mixed with corrosion inhibitors to adsorb corrosion inhibitor molecules, and then polyallyl ammonium chloride is added to form cationic corrosion inhibitors and SiO2 / ZrO2 nanoparticles, which are then mixed with corrosion inhibitors, and the above steps are repeated to prepare a mixed solution to obtain a layer-by-layer self-assembled multilayer film structure; the self-repairing coating prepared by the self-assembly method is not suitable for large-scale continuous production. Patent No. CN105001759B provides a molybdate-doped polypyrrole / epoxy resin self-healing coating and its preparation and application. Its defects are single-layer coating, corrosion inhibitor is evenly distributed in the organic coating, and no nano-container is used to encapsulate the corrosion inhibitor. Patent CN111909557A provides a self-healing capsule, self-healing anti-corrosion coating and its preparation method and application. Its defects are high resin solid content, coating dry film thickness of 100μm, and the coating takes up to one week to cure by room temperature drying, which is not suitable for efficient continuous production process.

[0004] In summary, the self-repairing coating disclosed in the prior art mainly adopts the method of directly adding corrosion inhibitors to resin coatings, and the resins also adopt traditional adhesive resins such as alkyd, phenolic, and epoxy; its main technical defect is that traditional resins lack self-crosslinking effect and cannot be re-crosslinked and repaired in a humid environment. Directly adding corrosion inhibitors to the coating, the corrosion inhibitors are not coated and loaded with nanocontainers, which will cause the corrosion inhibitors to act on the steel base when the coating is not damaged, resulting in a waste of corrosion inhibitors. Summary of the invention

[0005] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to continuously prepare a double-layer organic coating on the surface of galvanized steel strip by using a "coating-drying" two-coating and two-baking continuous production process: a self-repairing primer layer and a weather-resistant topcoat layer. Since nano-containers coated with corrosion inhibitors are added to the primer coating, the nano-containers have good sealing barrier properties under normal service conditions. When the primer coating of the color-coated plate is physically and mechanically damaged, the nano-containers at the damaged coating site can repair the damaged site by releasing corrosion inhibitors, and complete self-repair in a humid and water-seeping environment. The self-repairing property is due to the fact that the polyester polyurethane of the topcoat can interact with the corrosion inhibitor through reversible non-covalent bonds such as hydrogen bonds and ionic bonds in its molecular structure. When the material is damaged, these non-covalent bonds can be broken and reformed under appropriate conditions (such as temperature, humidity, etc.), thereby repairing the damaged part of the material.

[0006] In order to achieve the above-mentioned invention object, the present invention provides a method for producing a self-repairing color-coated steel plate for construction, which uses a "two-coating and two-baking" process for continuous production of color-coated steel plates to prepare color-coated steel plates having a self-repairing primer layer and a weather-resistant topcoat layer. The production method comprises the following steps:

[0007] ① The cleaned coated strip enters the continuous production entrance loop for roller coating pretreatment;

[0008] ② The pretreated coated steel strip enters the primer roller coater to dip the primer and back paint, then enters the primer curing furnace for drying, and water quenching and cooling to form a self-repairing primer layer and a back paint layer; the self-repairing primer layer is an epoxy resin containing a nanocontainer encapsulating a corrosion inhibitor, and the mass ratio of the nanocontainer added to the epoxy resin is 0.5% to 1%;

[0009] ③ The galvanized steel strip coated with primer is put into the topcoat roller coater to dip the topcoat, then enters the curing furnace for drying, water quenching and cooling to form a topcoat layer; finally, it is rolled into a roll through the outlet looper.

[0010] In the above technical solution, further, the metal substrate of the self-repairing color-coated steel plate for construction is preferably a galvanized, galvanized aluminum-magnesium or other coated steel plate.

[0011] Furthermore, the resin contained in the self-healing primer layer is an epoxy resin modified with a nanocontainer, wherein the nanocontainer is one of nanocontainers such as graphene oxide, MXene nanosheets, CeO2 hollow microspheres, MOF-5, ZIF-69, and ZIF-8.

[0012] Furthermore, the corrosion inhibitor contained in the self-repairing primer layer is a liquid hydrocarbon, such as anti-rust oil, oil-soluble corrosion inhibitor, for example, one of octadecylamine, benzotriazole, oleic acid imidazoline, 8-hydroxyquinoline, metal oxygen-containing salts (nitrites, vanadates, zirconates, molybdates), etc.

[0013] Furthermore, the epoxy resin contained in the self-repairing primer layer is one of bisphenol A epoxy resins E42, E44, and E51; the epoxy resin cross-linking curing agent is one of polyamide, maleic anhydride, phthalic anhydride, etc.; the epoxy resin cross-linking agent is one of phthalic acid, carbamate, formaldehyde resin, etc.

[0014] In the above technical solution, further, the topcoat layer of the self-repairing color-coated steel plate for construction is a polyurethane resin, including one of polyester polyurethane prepared by the reaction of polyester polyol and isocyanate, polyether polyurethane prepared by the reaction of polyether polyol and isocyanate, and aliphatic polyurethane synthesized using aliphatic isocyanate; in order to obtain the best self-repairing effect, polyester polyurethane prepared by the reaction of polyester polyol and isocyanate is preferred. The curing agent of the polyurethane resin of the topcoat layer is a tin compound, such as one of dioctyltin laurate, di-n-butyltin laurate, dibutyltin maleate, stannous octoate, etc.

[0015] Furthermore, the resin diluent of the back paint, primer and top paint of the self-repairing color-coated steel plate for construction is a mixed solvent of No. 200 solvent oil, xylene, ethyl acetate, butanol, acetone and the like.

[0016] Furthermore, the drying method of the self-repairing color-coated steel plate for construction is direct heating and drying and curing by gas (natural gas or coal gas), the drying and curing temperature is 100° C. to 120° C., and the curing time is 1 minute.

[0017] Furthermore, there are some differences in the pigments added to the primer and topcoat of the self-repairing color-coated steel plate for construction; wherein, the self-repairing primer layer adds anti-corrosion pigments, such as iron oxide red, zinc chrome yellow, carbon black, etc.; the polyurethane topcoat layer uses white, blue or green environmentally friendly material pigments, such as white pigments: talcum powder, titanium dioxide, barium sulfate, calcium carbonate, blue pigments: phthalocyanine blue, ultramarine blue, green pigments: iron oxide green, phthalocyanine green, chrome green, etc.

[0018] Furthermore, the thickener (anti-settling agent) in the primer and topcoat of the self-repairing color-coated steel plate for construction is one of polyvinyl alcohol, polyacrylic acid, hydroxyethyl cellulose, bentonite, montmorillonite, etc. The resin curing accelerator in the primer and topcoat is one of benzoyl peroxide, m-phenylenediamine, diaminodiphenylmethane, zinc cyclohexaneate, etc.

[0019] Furthermore, when the self-repairing color-coated steel plate is used as a building color-coated steel plate, the side facing the external environment is a self-repairing primer layer and a topcoat layer, and the other side facing the interior is a back paint single-layer color coating.

[0020] In the above technical scheme, further, the primer preparation process of the self-repairing color-coated steel plate for construction includes: first, adding the anti-settling agent and epoxy resin to the resin diluent, stirring and dissolving, and forming a stable epoxy resin diluent A; then preparing a nanocontainer dispersion B (corrosion inhibitor-nanocontainer / epoxy resin) loaded with a corrosion inhibitor; finally, 30wt% of the corrosion inhibitor-nanocontainer / epoxy resin, 40wt% of the diluent, 25wt% of the pigment and 5wt% of the additive are mixed and stirred to prepare the primer of the self-repairing color-coated steel plate. The primer component content of the self-repairing color-coated steel plate is shown in Table 1.

[0021] Furthermore, the nanocontainer solid powder encapsulating the corrosion inhibitor is obtained by centrifugation or filtration; and then the nanocontainer solid powder is evenly mixed with the epoxy resin diluent A to obtain the nanocontainer epoxy resin diluent containing the encapsulated corrosion inhibitor, that is, the corrosion inhibitor-loaded nanocontainer dispersion B (corrosion inhibitor-nanocontainer / epoxy resin).

[0022] Table 1 Primer component content of self-repairing color-coated steel plate

[0023]

[0024] In the above technical scheme, further, the topcoat of the self-repairing color-coated steel plate for construction is composed of 30wt% topcoat resin (polyester polyurethane), 40wt% solvent, 25wt% pigment and 5wt% additive; wherein, the polyester polyurethane is formed by the reaction of polyester polyol and polyisocyanate to form a cross-linked structure, which can give the paint film hardness, wear resistance and chemical resistance.

[0025] Further, the polyester polyol is synthesized by polycondensation reaction of polyacid (such as adipic acid, phthalic acid, etc.) and polyol (such as ethylene glycol, propylene glycol, etc.), with a molecular weight of 1000-3000; its mass ratio in the topcoat is 10%-15%. The polyisocyanate is toluene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI), which is a key component for forming a polyurethane paint film; its mass ratio in the topcoat is 10%-15%. The solvent is a mixed solvent of xylene, ethyl acetate, etc., used to dilute and dissolve polyester polyol and polyisocyanate, and its mass ratio in the topcoat is 30%-50%. The pigment is one of white, blue, and green environmentally friendly pigments, and its mass ratio in the topcoat is 25%. The additives include 0.5% defoamer, 1.5% curing accelerator, 2% anti-settling agent, and 1% leveling agent.

[0026] The coating of the self-repairing color-coated steel plate for construction consists of two layers, a self-repairing primer layer and a topcoat layer. The epoxy resin primer layer loaded with corrosion inhibitor nanocontainers mainly provides excellent bonding properties and loads corrosion inhibitors, and can release the corrosion inhibitors for self-repair when the coating is damaged; the topcoat layer is a polyester polyurethane made by reacting polyester polyol with isocyanate. The polyester resin structure in the polyester polyurethane coating has good stability and can resist erosion by natural factors such as ultraviolet radiation, temperature changes, and humidity changes; under long-term outdoor exposure environment, it can still maintain good color stability and glossiness, is not prone to fading, powdering, etc., and can effectively extend the service life of the color steel tile.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention utilizes the "two coating and two baking" process for the continuous production of color-coated steel plates to prepare color-coated steel plates with a self-repairing primer layer and a weather-resistant topcoat layer; the color-coated steel plates are not only environmentally friendly, corrosion-resistant, and highly decorative, but also self-repairing and can resist erosion by natural factors such as ultraviolet radiation, temperature changes, and humidity changes; they can be applied to the roofs and walls of buildings to provide protection and decorative functions for the buildings. The method is simple and convenient, can be produced continuously, and has high production efficiency; the technical advantages of the self-repairing color coating can improve the reliability of the material, reduce maintenance costs, extend service life, improve material performance, and adapt to complex environments, etc., and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the production process of the self-repairing color-coated steel plate of the present invention. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.

[0031] A method for producing a self-repairing color-coated steel plate for construction, the process flow is as follows Figure 1 The color coating process parameters are shown in Table 2, which specifically include the following steps:

[0032] ① The cleaned coated strip enters the continuous production entrance loop and is subjected to roller coating pretreatment (see Figure 1 Step 1 in

[0033] ② The pre-treated coated steel strip enters the primer roller coater to dip the primer and back paint, then enters the primer curing furnace for drying, water quenching and cooling to form a self-repairing primer layer and back paint layer (see Figure 1 Step 2); the self-repairing primer layer is an epoxy resin containing a nanocontainer encapsulating a corrosion inhibitor, and the mass ratio of the nanocontainer added to the epoxy resin is 0.5% to 1%;

[0034] ③ The galvanized steel strip coated with primer enters the topcoat roller coater to dip the topcoat, then enters the curing furnace for drying, water quenching and cooling to form a topcoat layer; finally, it is rolled into a roll through the outlet looper (see Figure 1 Step 3 in the above example).

[0035] Table 2 Color coating process parameters

[0036]

[0037] The matters not described in the following embodiments are the same as the description of the above specific implementation methods.

[0038] Example 1

[0039] A production method of a self-repairing color-coated steel plate for construction, the specific process flow is as follows:

[0040] The preparation process of self-repairing primer is as follows: ① Add 5 parts of 8-hydroxyquinoline to 10 parts of graphene oxide nano-slurry, stir and mix evenly, and then filter out the graphene oxide nano-sheets loaded with 8-hydroxyquinoline corrosion inhibitor. ② 30wt% E51 epoxy resin, 40wt% toluene, xylene, Solvesso150 aromatic hydrocarbon mixed solvent, 25wt% paint pigment and 5wt% paint additives loaded with graphene oxide nano-sheets loaded with corrosion inhibitor are used as self-repairing primer layer. Then the strip enters the primer curing furnace for curing at 210℃ for 30s, and the strip runs at a speed of 60m / min to prepare a primer coating with a thickness of 5 to 6μm.

[0041] The production process of the color-coated plate topcoat is as follows: the strip enters the topcoat roller coater, and the topcoat contains 30wt% polyester polyurethane, 40wt% butyl acetate, xylene, acetone mixed solvent, 25wt% pigment and 5wt% paint additive. Then it enters the topcoat curing furnace and bakes at 250°C for 30s to cure the topcoat, prepare a polyurethane topcoat layer, and finally manufacture a self-repairing color steel coil finished product; the coating performance test results of the finished product obtained in Example 1 are shown in Table 3.

[0042] Example 2

[0043] A production method of a self-repairing color-coated steel plate for construction, the specific process flow is as follows:

[0044] The preparation process of the self-repair primer is as follows: ① Dissolve 1.5 parts by mass of Zn(NO3)·6H2O in 200 parts by mass of deionized water, and dissolve 6.5 parts by mass of 2-methylimidazole in 200 parts by mass of deionized water; then add the zinc nitrate solution dropwise to the 2-methylimidazole solution under stirring. After stirring for 24 hours, the white ZIF-8 product was collected by centrifugation at 10000rpm, and then washed with deionized water three times. ② Add the white ZIF-8 powder to 1g / L sodium nitrite solution and stir at 600rmp for 36 hours to complete the adsorption and loading of sodium nitrite. Filter out the ZIF-8 powder loaded with sodium nitrate. ③ The E42 epoxy resin 30wt% of ZIF-8 loaded with corrosion inhibitor, 40wt% of toluene, xylene, Solvesso150 aromatic hydrocarbon mixed solvent, 25wt% paint pigment and 5wt% paint additive are used as the self-repair primer layer. The strip then enters a primer curing furnace for curing at 210°C for 30 seconds with a strip running speed of 60m / min to prepare a primer coating with a thickness of 5-6μm.

[0045] Color-coated plate topcoat production process: The steel strip enters the topcoat roller coater, and the topcoat contains 30wt% polyester polyurethane, 40wt% butyl acetate, xylene, acetone mixed solvent, 25wt% pigment and 5wt% paint additive. Then it enters the topcoat curing furnace to bake at 250℃ for 30s to cure the topcoat, prepare the polyurethane topcoat layer, and finally manufacture the self-repairing color-coated steel coil finished product; the coating performance test results of the finished product obtained in Example 2 are shown in Table 3.

[0046] Example 3

[0047] A production method of a self-repairing color-coated steel plate for construction, the specific process flow is as follows:

[0048] The preparation process of self-repairing primer is as follows: ① Dissolve 6 parts by mass of zinc nitrate hexahydrate in 20 parts by mass of deionized water, and 1 part by mass of terephthalic acid in 20 parts by mass of N,N-dimethylformamide. Mix the two solutions and place them in a high-pressure reactor to react at 180°C for 24 hours, and collect the MOF-5 nanoparticles formed in the solution. ② Add white ZIF-8 powder to 1g / L zinc gluconate solution and stir at 600rmp for 36 hours to complete the adsorption and loading of zinc gluconate. Filter out the MOF-5 powder loaded with zinc gluconate. ③ The MOF-5 loaded with corrosion inhibitor, 30wt% of E41 epoxy resin, 40wt% of xylene, butanol, butanone mixed solvent, 25wt% paint pigment and 5wt% paint additive are used as self-repairing primer layer. Then the strip enters the primer curing furnace for curing at 210°C for 30s, and the strip runs at a speed of 60m / min to prepare a primer coating with a thickness of 5 to 6μm.

[0049] Color-coated plate topcoat production process: The strip enters the topcoat roller coater, and the topcoat contains 30wt% polyester polyurethane, 40wt% butyl acetate, xylene, acetone mixed solvent, 25wt% pigment and 5wt% paint additive. Then it enters the topcoat curing furnace to bake at 250℃ for 30s to cure the topcoat, prepare the polyurethane topcoat layer, and finally manufacture the self-repairing color-coated steel coil finished product; the coating performance test results of the finished product obtained in Example 3 are shown in Table 3.

[0050] Example 4

[0051] A production method of a self-repairing color-coated steel plate for construction, the specific process flow is as follows:

[0052] The production process of self-priming low-repair paint is as follows: ① Take 1 part by mass of cerium nitrate hexahydrate and 6g of maleic hydrazide, pour them into a test tube containing 150 parts by mass of N,N-dimethylformamide solvent, ultrasonically dissolve for 20 minutes, and wait for the solid particles to be completely dissolved. Then transfer the solution to a high-pressure reactor, react at 170°C for 15 minutes to obtain an orange solution, centrifuge and wash the solution, and harvest the orange Ce-MOF. ② Add the orange Ce-MOF powder to 1g / L sodium molybdate solution, stir at 600rmp for 36h, and complete the adsorption and loading of sodium molybdate. Filter out the Ce-MOF powder loaded with sodium molybdate. ③ The E44 epoxy resin of Ce-MOF loaded with sodium molybdate corrosion inhibitor 30wt%, 40wt% of xylene, toluene, butanone mixed solvent, 25wt% paint pigment and 5wt% paint additive are used as a self-repairing primer layer. The strip then enters a primer curing furnace for curing at 210°C for 30 seconds with a strip running speed of 60m / min to prepare a primer coating with a thickness of 5 to 6μm.

[0053] Color-coated plate topcoat production process: The strip enters the topcoat roller coater, and the topcoat contains 30wt% polyester polyurethane, 40wt% butyl acetate, xylene, acetone mixed solvent, 25wt% pigment and 5wt% paint additive. Then it enters the topcoat curing furnace and bakes at 250℃ for 30s to cure the topcoat, prepare the polyurethane topcoat layer, and finally manufacture the self-repairing color-coated steel coil finished product; the coating performance test results of the finished product obtained in Example 4 are shown in Table 3.

[0054] Comparative Example 1

[0055] Ordinary commercial paint is used to make color-coated steel plates, and the primer coating of the color-coated steel plates does not contain nano-containers loaded with corrosion inhibitors.

[0056] The color-coated plate cross-drawing test is used to compare the corrosion resistance and self-repair performance of the color-coated plate. When conducting the color-coated plate cross-drawing test, follow the following steps (refer to GB / T 13448-2019 "Test methods for color-coated steel plates and steel strips"):

[0057] Prepare the sample: The sample size is generally 75mm×150mm, the surface should be flat, free of oil, damage, and burrs on the edge. The number of samples of the same type should be no less than 3. Before the test, two intersecting straight lines are drawn on the sample along the diagonal direction. The lines should penetrate the coating. After 48 hours of neutral salt spray test, the corrosion propagation distance of the scratched part of the sample is measured. The performance comparison of the coating of the embodiment and the comparative example is shown in Table 3.

[0058] Table 3 Comparison of coating properties of the embodiments and comparative examples

[0059] 48h cross test corrosion Corrosion resistance Self-healing Nano container Example 1 No corrosion Excellent √ Graphene oxide Example 2 No corrosion Excellent √ ZIF-8 Example 3 No corrosion Excellent √ MOF-5 Example 4 No corrosion Excellent √ Ce-MOF Comparative Example 1 White rust on the scratched part have / /

[0060] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0061] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0062] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for producing a self-repairing color-coated steel plate for construction, characterized in that: The production method comprises the following steps: ① The cleaned coated strip enters the continuous production entrance loop for roller coating pretreatment; ② The pretreated coated steel strip enters the primer roller coater to dip the primer and back paint, then enters the primer curing furnace for drying, and water quenching and cooling to form a self-repairing primer layer and a back paint layer; the self-repairing primer layer is an epoxy resin containing a nanocontainer encapsulating a corrosion inhibitor, and the mass ratio of the nanocontainer added to the epoxy resin is 0.5% to 1%; ③ The galvanized steel strip coated with primer is put into the topcoat roller coater to dip the topcoat, then enters the curing furnace for drying, water quenching and cooling to form a topcoat layer; finally, it is rolled into a roll through the outlet looper.

2. The production method according to claim 1, characterized in that The resin contained in the self-repairing primer layer is a modified epoxy resin with added nanocontainers, wherein the nanocontainers are one of graphene oxide, MXene nanosheets, CeO2 hollow microspheres, MOF-5, ZIF-69, and ZIF-8.

3. The production method according to claim 1, characterized in that The corrosion inhibitor contained in the self-repairing primer layer is one of octadecylamine, benzotriazole, oleic acid imidazoline, 8-hydroxyquinoline, and metal oxygen acid salt.

4. The production method according to claim 1, characterized in that The epoxy resin contained in the self-repairing primer layer is one of bisphenol A epoxy resins E42, E44, and E51; the epoxy resin cross-linking curing agent is one of polyamide, maleic anhydride, and phthalic anhydride; the epoxy resin cross-linking agent is one of phthalic acid, carbamate, and formaldehyde resin.

5. The production method according to claim 1, characterized in that: The topcoat layer of the self-repairing color-coated steel plate for construction is a polyurethane resin, preferably a polyester polyurethane made by reacting polyester polyol with isocyanate; the curing agent of the polyurethane resin is a tin compound, which is one of dioctyltin laurate, di-n-butyltin laurate, dibutyltin maleate, and stannous octoate.

6. The production method according to claim 1, characterized in that: The primer preparation process of the self-repairing color-coated steel plate for construction comprises: firstly, adding an anti-settling agent and an epoxy resin into a resin diluent, stirring and dissolving, and forming a stable epoxy resin diluent; then preparing a nano-container dispersion liquid loaded with a corrosion inhibitor, i.e., a corrosion inhibitor-nano-container / epoxy resin; and finally, mixing and stirring 30 wt % of the corrosion inhibitor-nano-container / epoxy resin, 40 wt % of a diluent, 25 wt % of a pigment, and 5 wt % of an additive, and preparing the primer of the self-repairing color-coated steel plate.

7. The production method according to claim 1, characterized in that: The topcoat of the self-repairing color-coated steel plate for construction consists of 30 wt% of polyester polyurethane, 40 wt% of solvent, 25 wt% of pigment and 5 wt% of additive.

Citation Information

Cited By

  • Heavy-duty anti-corrosion coating with corrosion inhibition and self-healing synergistic effect and preparation method of heavy-duty anti-corrosion coating

    CN120005504A

  • A heavy-duty anticorrosive coating with synergistic effect of corrosion inhibition and self-healing and a preparation method thereof

    CN120005504B

  • Self-repairing coating material based on MOFs, preparation method and application of self-repairing coating material to paint surface protective film

    CN122563468A