High-solid-content nanoparticle quick-drying ink, preparation method and part preparation method
Through the fast-drying ink and laser melting process of high solid content nanoparticles, the problems of complex process, time-consuming and low yield in adhesive jet forming technology are solved, and efficient and precise additive manufacturing is achieved, suitable for a variety of materials and industrial sectors.
Patent Information
- Application Number
- CN202410968068.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-12-03
AI Technical Summary
The existing adhesive jet forming technology is complex and time-consuming, with low yield and low dimensional accuracy, which limits its wide application in industry.
Using high-solid content nanoparticle quick-drying ink and laser melting technology, the manufacturing process is simplified through two main steps: jet printing and laser melting, ensuring the stability of the blank shape, and accelerating the solidification and CO2 laser melting through infrared light or heat source to achieve high curing Accurate molding.
Simplify the process flow, improve yield and dimensional accuracy, is suitable for a variety of nanoparticle materials, has a wide range of industrial application prospects, and is suitable for aerospace, automobile manufacturing, and biomedicine.
Smart Images

Figure CN119057058A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a high-solid content nanoparticle quick-drying ink, a preparation method and a parts preparation method. Background Art
[0002] Additive Manufacturing (AM) is an advanced manufacturing technology that has developed rapidly in recent years. It can manufacture parts with complex geometric shapes by stacking materials layer by layer. Traditional additive manufacturing technologies include stereolithography (SLA), selective laser sintering (SLS), fused deposition modeling (FDM), and binder jetting. These technologies have their own advantages, but there are still many challenges and shortcomings in practical applications.
[0003] Among them, the binder jet forming technology uses a binder to bind powder materials layer by layer, and then needs to go through multiple steps such as curing, de-powdering and sintering to obtain the final parts. This series of steps is not only complex and time-consuming, but also prone to problems such as powder residue, low dimensional accuracy and low yield during the de-powdering and sintering process, which seriously limits the widespread application of this technology in industry.
[0004] In order to overcome these shortcomings, a new additive manufacturing method is urgently needed that can simplify the process flow, improve the yield and dimensional accuracy. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high-solid content nanoparticle quick-drying ink, a preparation method and a method for preparing parts. The present invention solves the problems of complex process, long time consumption, low dimensional accuracy and low yield rate in the existing binder jet forming technology. By simplifying the process flow and improving the yield and dimensional accuracy of parts, efficient and precise additive manufacturing is achieved.
[0006] The present invention adopts the following technical solution:
[0007] In one aspect, the present invention provides a method for preparing a high-solid content nanoparticle quick-drying ink, comprising:
[0008] S1, mixing the precursor, nanoparticles and quick-drying solvent in a set ratio to obtain a basic solution;
[0009] S2, adding a dispersant to uniformly disperse the nanoparticles in the base solution to form a uniform suspension;
[0010] S3, filtering to remove large particles and impurities in the suspension to obtain the high solid content nanoparticle quick-drying ink.
[0011] According to the above aspects and any possible implementation, there is further provided an implementation, in step S1, the precursor includes copper salt, iron salt, aluminum salt and zirconium salt.
[0012] According to the aspects described above and any possible implementation, an implementation is further provided, wherein the copper salt comprises a mixture of one or more of copper formate, copper acetate, copper citrate, copper acetylacetonate, copper perchlorate, copper chloride, and copper sulfate; the iron salt comprises a mixture of one or more of iron formate, iron acetate, iron citrate, iron nitrate, iron acetylacetonate, iron perchlorate, iron chloride, and iron sulfate; the aluminum salt comprises a mixture of one or more of aluminum formate, aluminum acetate, aluminum citrate, aluminum nitrate, aluminum acetylacetonate, aluminum perchlorate, aluminum chloride, and aluminum sulfate; the zirconium salt comprises a mixture of one or more of zirconium formate, zirconium acetate, zirconium citrate, zirconium nitrate, zirconium acetylacetonate, zirconium perchlorate, zirconium chloride, and zirconium sulfate.
[0013] According to the aspects and any possible implementation methods described above, an implementation method is further provided. In step S1, the nanoparticles include one or more of copper nanoparticles (1-300nm), iron nanoparticles (1-300nm), aluminum oxide nanoparticles (1-300nm), zirconium oxide nanoparticles (1-300nm), and titanium oxide (5-100nm) nanoparticles.
[0014] According to the above aspects and any possible implementations, an implementation is further provided, in which the nanoparticles are uniformly dispersed in the base solution by ultrasonic dispersion or ball milling.
[0015] According to the aspects described above and any possible implementation method, an implementation method is further provided. In step S2, the quick-drying solvent includes one of methanol, ethanol, and isopropanol; the dispersant includes a surfactant dispersant, a polymer dispersant, a small molecule organic compound dispersant, a small molecule inorganic salt dispersant, and an amphoteric dispersant.
[0016] According to the above aspects and any possible implementation, an implementation is further provided, wherein the surfactant dispersant comprises one of sodium dodecyl sulfate (SDS), alkyl sulfonates, cetyltrimethylammonium bromide (CTAB), benzyltrimethylammonium chloride, polyethylene glycol (PEG), polyoxyethylene ether (Triton X-100) and fatty alcohol polyoxyethylene ether;
[0017] The polymer dispersant includes one of polyvinyl pyrrolidone (PVP), sodium polyacrylate, sodium carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyethylene oxide (PEO) and polyacrylate;
[0018] The small molecule organic compound dispersant includes one of citric acid, tartaric acid, and carbamate;
[0019] The small molecule inorganic salt dispersant includes one of sodium hexametaphosphate (SHMP), sodium tripolyphosphate (STPP), and sodium pyrophosphate;
[0020] The amphoteric dispersants include, but are not limited to, lecithin and phosphatidylcholine.
[0021] According to the above aspects and any possible implementation, an implementation is further provided, in step S1, the ratio of the precursor, nanoparticles, and quick-drying solvent is: 10-20wt.% of the precursor, 40-70wt.% of the nanoparticles, and the balance is the quick-drying solvent.
[0022] On the other hand, the present invention also provides a high-solid content nanoparticle quick-drying ink, which is obtained by the above-mentioned high-solid content nanoparticle quick-drying ink preparation method, and the solid content of the quick-drying ink is 50-70wt.%.
[0023] On the other hand, the present invention also provides a method for preparing parts by spraying high-solid content nanoparticle quick-drying ink and laser melting, wherein the quick-drying ink is obtained by the above-mentioned high-solid content nanoparticle quick-drying ink preparation method, and the method for preparing parts comprises:
[0024] X1. Jet printing blank:
[0025] X11, using an inkjet printing device to spray the prepared quick-drying ink layer by layer along a predetermined path to form a blank;
[0026] X12. After each layer is sprayed, the ink is cured by an infrared light source or a heat source;
[0027] X2, laser melting: Use CO2 laser or fiber laser to melt the printed blank layer by layer, adjust the energy density and scanning path of the laser according to the material characteristics of the blank to ensure uniform melting;
[0028] X3. Post-processing: Mechanically clean the parts after laser melting to remove surface residues; then polish them to improve the surface finish.
[0029] According to the aspects and any possible implementations described above, an implementation is further provided, in step X12, the curing time does not exceed 10 seconds, and the thickness of each layer of the green body is controlled between 10-100 μm.
[0030] The beneficial effects of the present invention are:
[0031] 1. Simplified process flow: Traditional binder jet forming technology requires multiple steps such as printing, curing, de-powdering and sintering. However, the method of the present invention uses high-solid content nanoparticle quick-drying ink and laser melting process, which only requires two main steps: printing and melting, greatly simplifying the manufacturing process.
[0032] 2. Improve yield and dimensional accuracy: Quick-drying ink solidifies quickly after spraying, ensuring the shape of the blank is stable, thereby reducing the problems of low yield and low dimensional accuracy caused by the de-powdering and sintering steps in the traditional process. The energy density and scanning path during the laser melting process can be precisely adjusted according to the material properties and geometric shape to ensure uniform melting and high-precision molding of the parts.
[0033] 3. Multi-material applicability: By adjusting the formula of the quick-drying ink and the laser melting parameters, the method of the present invention can be adapted to a variety of nanoparticle materials (such as nano-copper, nano-iron, aluminum oxide, zirconium oxide, etc.) and has a wide range of material applicability.
[0034] 4. Broad industrial application prospects: The parts manufactured by the method of the present invention have broad application prospects in the fields of aerospace, automobile manufacturing, biomedicine, etc., and can meet the demand for high-performance and high-precision parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The figure is a schematic flow chart of a method for preparing a high solid content nanoparticle quick-drying ink according to an embodiment of the present invention. DETAILED DESCRIPTION
[0036] The specific embodiments of the present invention will be described in detail below in conjunction with specific drawings. It should be noted that the technical features or combinations of technical features described in the following embodiments should not be considered isolated, and they can be combined with each other to achieve better technical effects.
[0037] like Figure 1 As shown, a method for preparing a high-solid content nanoparticle quick-drying ink according to an embodiment of the present invention comprises:
[0038] S1, mixing the precursor, nanoparticles and quick-drying solvent in a set ratio to obtain a basic solution;
[0039] S2, adding a dispersant to uniformly disperse the nanoparticles in the base solution to form a uniform suspension;
[0040] S3, filtering to remove large particles and impurities in the suspension to obtain the high solid content nanoparticle quick-drying ink.
[0041] According to the above aspects and any possible implementation, there is further provided an implementation, in step S1, the precursor includes copper salt, iron salt, aluminum salt and zirconium salt.
[0042] In a specific embodiment, the copper salt includes a mixture of one or more of copper formate, copper acetate, copper citrate, copper acetylacetonate, copper perchlorate, copper chloride, and copper sulfate; the iron salt includes a mixture of one or more of iron formate, iron acetate, iron citrate, iron nitrate, iron acetylacetonate, iron perchlorate, iron chloride, and iron sulfate; the aluminum salt includes a mixture of one or more of aluminum formate, aluminum acetate, aluminum citrate, aluminum nitrate, aluminum acetylacetonate, aluminum perchlorate, aluminum chloride, and aluminum sulfate; the zirconium salt includes a mixture of one or more of zirconium formate, zirconium acetate, zirconium citrate, zirconium nitrate, zirconium acetylacetonate, zirconium perchlorate, zirconium chloride, and zirconium sulfate.
[0043] In a specific embodiment, in step S1, the nanoparticles include one or more of copper nanoparticles (1-300nm), iron nanoparticles (1-300nm), aluminum oxide nanoparticles (1-300nm), zirconium oxide nanoparticles (1-300nm), and titanium oxide (5-100nm) nanoparticles.
[0044] In a specific embodiment, the nanoparticles are uniformly dispersed in the base solution by ultrasonic dispersion or ball milling.
[0045] In a specific embodiment, in step S2, the quick-drying solvent includes one of methanol, ethanol, and isopropanol; the dispersant includes surfactant dispersants, polymer dispersants, small molecule organic compound dispersants, small molecule inorganic salt dispersants and amphoteric dispersants.
[0046] In a specific embodiment, the surfactant dispersant includes one of sodium dodecyl sulfate (SDS), alkyl sulfonates, cetyltrimethylammonium bromide (CTAB), benzyltrimethylammonium chloride, polyethylene glycol (PEG), polyoxyethylene ether (Triton X-100) and fatty alcohol polyoxyethylene ether.
[0047] In a specific embodiment, the polymer dispersant includes one of polyvinyl pyrrolidone (PVP), sodium polyacrylate, sodium carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyethylene oxide (PEO) and polyacrylate;
[0048] In a specific embodiment, the small molecule organic compound dispersant includes one of citric acid, tartaric acid, and carbamate.
[0049] In a specific embodiment, the small molecule inorganic salt dispersant includes one of sodium hexametaphosphate (SHMP), sodium tripolyphosphate (STPP), and sodium pyrophosphate.
[0050] In a specific embodiment, the amphoteric dispersant includes but is not limited to lecithin and phosphatidylcholine.
[0051] In a specific implementation, in step S1, the ratio of the precursor, nanoparticles, and quick-drying solvent is: 10-20wt.% of the precursor, 40-70wt.% of the nanoparticles, and the balance of the quick-drying solvent. This ratio setting can maximize the solid content in the binder, so that the strength of the part after the binder is sprayed is high, which is conducive to the next stage of laser melting.
[0052] On the other hand, an embodiment of the present invention provides a high-solid content nanoparticle quick-drying ink, which is obtained by the above-mentioned high-solid content nanoparticle quick-drying ink preparation method, and the solid content of the quick-drying ink is 50-70wt.%.
[0053] On the other hand, an embodiment of the present invention provides a method for preparing a part by spraying a high-solid content nanoparticle quick-drying ink and laser melting, wherein the quick-drying ink is obtained by using the above-mentioned method for preparing a high-solid content nanoparticle quick-drying ink. The method for preparing a part comprises:
[0054] X1. Jet printing blank:
[0055] X11, using an inkjet printing device to spray the prepared quick-drying ink layer by layer along a predetermined path to form a blank;
[0056] X12. After each layer is sprayed, the ink is cured by an infrared light source or a heat source;
[0057] X2, laser melting: Use CO2 laser or fiber laser to melt the printed blank layer by layer, adjust the energy density and scanning path of the laser according to the material characteristics of the blank to ensure uniform melting;
[0058] X3. Post-processing: Mechanically clean the parts after laser melting to remove surface residues; then polish them to improve the surface finish.
[0059] In a specific embodiment, in step X12, the curing time does not exceed 10 seconds to ensure the stability of the shape of each layer of the green body; the thickness of each layer of the green body is controlled between 10-100 μm.
[0060] The present invention uses 10-20wt.% of organic salt and inorganic salt components and a specific dispersant to form nanoparticles into micelles, which are stably dispersed in a quick-drying ink system to prepare a high-solid content ink (40-70wt.%).
[0061] Compared with traditional binder jet forming technology, this method only requires two main steps: "jet printing the blank" and "laser melting", realizing an one-piece formed product and simplifying the entire manufacturing process.
[0062] The use of an infrared light source or a heat source combined with a low-boiling point solvent ensures that the curing time does not exceed 10 seconds, ensuring the shape stability of the printed body.
[0063] Example 1
[0064] A high solid content copper nanoparticle quick-drying ink, the specific preparation process is as follows:
[0065] (1) mixing 10 wt.% copper acetate, 50 wt.% nano copper particles (particle size 1-100 nm) and a methanol-ethanol mixture to form a base solution;
[0066] (2) adding sodium dodecyl sulfate (SDS) and dispersing it for 30 min using an ultrasonic dispersing device to uniformly disperse the nano-copper particles in the solvent to form a uniform suspension;
[0067] (3) Filter through a 0.2 μm filter membrane to remove large particles and impurities to obtain a nano copper particle quick-drying ink with a high solid content. The printing process is as follows: Use an inkjet printing device to spray the quick-drying ink layer by layer along a predetermined path. After each layer is sprayed, an infrared light source is used to accelerate the curing of the ink, and the curing time does not exceed 10 seconds; the layer thickness is set to 50 μm, thereby constructing a blank;
[0068] The melting steps are as follows: Use a CO2 laser to melt the printed blank layer by layer, adjust the laser power to 300W, and the scanning rate to 10mm / s to ensure uniform melting of the blank.
[0069] Finally, use ultrasonic cleaning equipment to remove residues on the surface of the parts, and use a polishing machine to polish the surface of the parts to improve the surface finish.
[0070] Example 2
[0071] A high solid content aluminum oxide nanoparticle quick-drying ink, the specific preparation process is as follows:
[0072] (1) 13 wt.% aluminum acetate, 60 wt.% nano-alumina particles (particle size 50-200 nm) and 25 wt.% isopropanol were mixed to form a base solution;
[0073] (2) adding 2 wt.% polyethylene glycol (PEG) and dispersing it using a ball mill for 2 h to uniformly disperse the nano-alumina particles in the solvent to form a uniform suspension;
[0074] (3) Filter through a 0.1 μm filter membrane to remove large particles and impurities to obtain a high solid content nano-aluminum oxide particle quick-drying ink.
[0075] The printing process is as follows: use an inkjet printing device to spray quick-drying ink layer by layer along a predetermined path. After each layer is sprayed, an infrared light source is used to accelerate the curing of the ink, and the curing time does not exceed 8 seconds. The layer thickness is set to 30 μm, thereby constructing a blank.
[0076] The melting steps are as follows: Use a CO2 laser to melt the printed blank layer by layer, adjust the laser power to 600W, and the scanning rate to 8mm / s to ensure uniform melting of the blank.
[0077] Finally, use ultrasonic cleaning equipment to remove residues on the surface of the parts, and use a polishing machine to polish the surface of the parts to improve the surface finish.
[0078] Example 3
[0079] A high solid content zirconium oxide nanoparticle quick-drying ink, the specific preparation process is as follows:
[0080] (1) 9 wt.% zirconium citrate, 55 wt.% nano zirconium oxide particles (particle size 10-150 nm) and 33 wt.% methanol were mixed to form a base solution;
[0081] (2) adding 3 wt.% sodium carboxymethyl cellulose (CMC) and dispersing it for 45 min using an ultrasonic dispersing device to uniformly disperse the nano zirconium oxide particles in the solvent to form a uniform suspension;
[0082] (3) Filter through a 0.2 μm filter membrane to remove large particles and impurities to obtain a high-solid content nano-zirconia particle quick-drying ink.
[0083] The printing process is as follows: use an inkjet printing device to spray quick-drying ink layer by layer along a predetermined path. After each layer is sprayed, an infrared light source is used to accelerate the curing of the ink, and the curing time does not exceed 9 seconds. The layer thickness is set to 25μm, thereby constructing a blank;
[0084] The melting steps are as follows: Use a CO2 laser to melt the printed blank layer by layer, adjust the laser power to 500W, and the scanning rate to 8mm / s to ensure uniform melting of the blank.
[0085] Finally, use ultrasonic cleaning equipment to remove residues on the surface of the parts, and use a polishing machine to polish the surface of the parts to improve the surface finish.
[0086] The present invention uses nanoparticles with high solid content (such as nano copper, nano iron, aluminum oxide and zirconium oxide, etc.) to prepare quick-drying ink. The solid content of the ink can reach 50-70wt.%, and by adding quick-drying solvents and dispersants, the ink is ensured to solidify quickly within a short time after spraying. The high-solid content nanoparticle quick-drying ink is sprayed along a predetermined path using an inkjet printing device, and is stacked layer by layer to form a blank. The quick-drying ink solidifies quickly after spraying, ensuring that the shape of each layer of the blank is stable. The printed blank is melted layer by layer by a high-precision laser. The energy density and scanning path of the laser can be adjusted according to the material properties and geometric shape of the blank to ensure uniform melting and final molding of the blank. The blank after laser melting does not need to undergo traditional de-powdering and sintering steps, and only simple cleaning and surface treatment are required to obtain the final part.
[0087] Although several embodiments of the present invention have been given herein, those skilled in the art should understand that the embodiments of the present invention may be modified without departing from the spirit of the present invention. The above embodiments are merely exemplary and should not be used as a limitation on the scope of the present invention.
Claims
1. A method for preparing high solid content nanoparticle quick-drying ink, characterized in that: The method comprises: S1, mixing the precursor, nanoparticles and quick-drying solvent in a set ratio to obtain a basic solution; S2, adding a dispersant to uniformly disperse the nanoparticles in the base solution to form a uniform suspension; S3, filtering to remove large particles and impurities in the suspension to obtain the high solid content nanoparticle quick-drying ink.
2. The method for preparing the high solid content nanoparticle quick-drying ink according to claim 1, characterized in that: In step S1, the precursor includes copper salt, iron salt, aluminum salt and zirconium salt.
3. The method for preparing the high solid content nanoparticle quick-drying ink according to claim 2, characterized in that: The copper salt includes a mixture of one or more of copper formate, copper acetate, copper citrate, copper acetylacetonate, copper perchlorate, copper chloride, and copper sulfate; the iron salt includes a mixture of one or more of iron formate, iron acetate, iron citrate, iron nitrate, iron acetylacetonate, iron perchlorate, iron chloride, and iron sulfate; the aluminum salt includes a mixture of one or more of aluminum formate, aluminum acetate, aluminum citrate, aluminum nitrate, aluminum acetylacetonate, aluminum perchlorate, aluminum chloride, and aluminum sulfate; the zirconium salt includes a mixture of one or more of zirconium formate, zirconium acetate, zirconium citrate, zirconium nitrate, zirconium acetylacetonate, zirconium perchlorate, zirconium chloride, and zirconium sulfate.
4. The method for preparing a high solid content nanoparticle quick-drying ink according to claim 1, characterized in that: In step S1, the nanoparticles include one or more of copper nanoparticles, iron nanoparticles, aluminum oxide nanoparticles, zirconium oxide nanoparticles, and titanium oxide nanoparticles.
5. The method for preparing the high solid content nanoparticle quick-drying ink according to claim 1, characterized in that: In step S2, the quick-drying solvent includes one of methanol, ethanol, and isopropanol; the dispersant includes surfactant dispersants, polymer dispersants, small molecule organic compound dispersants, small molecule inorganic salt dispersants, and amphoteric dispersants.
6. The method for preparing the high solid content nanoparticle quick-drying ink according to claim 5, characterized in that: The surface active dispersant includes one of sodium dodecyl sulfate (SDS), alkyl sulfonate, cetyltrimethylammonium bromide (CTAB), benzyltrimethylammonium chloride, polyethylene glycol (PEG), polyoxyethylene ether (Triton X-100) and fatty alcohol polyoxyethylene ether; The polymer dispersant includes one of polyvinyl pyrrolidone (PVP), sodium polyacrylate, sodium carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyethylene oxide (PEO) and polyacrylate; The small molecule organic compound dispersant includes one of citric acid, tartaric acid, and carbamate; The small molecule inorganic salt dispersant includes one of sodium hexametaphosphate (SHMP), sodium tripolyphosphate (STPP), and sodium pyrophosphate; The amphoteric dispersants include, but are not limited to, lecithin and phosphatidylcholine.
7. The method for preparing a high solid content nanoparticle quick-drying ink according to claim 1, characterized in that: In step S1, the ratio of the precursor, nanoparticles and quick-drying solvent is: 10-20 wt.% of the precursor, 40-70 wt.% of the nanoparticles, and the balance is the quick-drying solvent.
8. A high solid content nanoparticle quick-drying ink, characterized in that: The quick-drying ink is obtained by the method for preparing a high-solid-content nanoparticle quick-drying ink according to any one of claims 1 to 7, and the solid content of the quick-drying ink is 50-70 wt.%.
9. A method for preparing parts by spraying high-solid content nanoparticle quick-drying ink and laser melting, characterized in that: The quick-drying ink is obtained by using the method for preparing the quick-drying ink with high solid content nanoparticles according to any one of claims 1 to 7, and the method for preparing the parts comprises: X1. Jet printing blank: X11, using an inkjet printing device to spray the prepared quick-drying ink layer by layer along a predetermined path to form a blank; X12. After each layer is sprayed, the ink is cured by an infrared light source or a heat source; X2, laser melting: Use CO2 laser or fiber laser to melt the printed blank layer by layer, adjust the energy density and scanning path of the laser according to the material characteristics of the blank to ensure uniform melting; X3. Post-processing: Mechanically clean the parts after laser melting to remove surface residues; then polish them to improve the surface finish.
10. The method for preparing parts by spraying high-solid content nanoparticle quick-drying ink and laser melting as claimed in claim 9, characterized in that: In step X12, the curing time does not exceed 10 seconds, and the thickness of each layer of the green body is controlled between 10-100 μm.