Low-oxygen-content porous titanium diffusion layer and preparation method thereof
By wrapping the zirconia ceramic plate and molybdenum plate, the contact between the titanium thin strip green body and oxygen is avoided, and a porous titanium diffusion layer is successfully prepared, which solves the oxygen pollution problem and improves the porous titanium diffusion layer. Mechanical strength and conductivity.
Patent Information
- Application Number
- CN202411256053.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
AI Technical Summary
The existing porous titanium diffusion layer is prone to introduce oxygen contamination during the preparation process, resulting in an increase in oxygen content, thereby reducing mechanical strength and electrical conductivity.
By rolling titanium powder into thin strip green body and wrapping it between zirconia ceramic plate and molybdenum plate to avoid contact between the titanium thin strip green body and oxygen, a low-oxygen content porous titanium diffusion layer was prepared by vacuum sintering.
The oxygen content of the porous titanium diffusion layer is effectively reduced, its mechanical strength and electrical conductivity are improved, and the preparation of the porous titanium diffusion layer with low oxygen content and high porosity is ensured.
Smart Images

Figure CN119057069A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen production by electrolysis of water, and in particular relates to a low-oxygen content porous titanium diffusion layer and a preparation method thereof. Background Art
[0002] The porous diffusion layer is the core component of the proton exchange membrane (PEM) water electrolysis hydrogen production device. Its materials, structure, design and preparation method play a key role in further improving the performance and efficiency of electrolytic hydrogen production and reducing costs. On the anode side, water enters the membrane electrode surface through the PEM for decomposition reaction, releasing oxygen molecules, protons and electrons. Since the environment inside the PEM water electrolysis cell is acidic and the applied voltage is higher than 1.5V, it causes high oxygen evolution potential and oxidative active oxygen generated during water electrolysis, as well as chemical and electrochemical corrosion in the acidic environment, making the traditional carbon materials (carbon paper, carbon cloth) and ordinary metal materials (stainless steel felt, nickel mesh, etc.) used in fuel cells no longer suitable for anode porous diffusion layer materials.
[0003] At present, titanium with good corrosion resistance is generally used as the diffusion layer material of PEM (proton exchange membrane) water electrolyzer. Among them, porous titanium diffusion layer has become one of the products with the most development potential due to its advantages such as high mechanical stability, high controllability of pore structure and good conductivity. However, the porous titanium diffusion layer has a large specific surface area and the preparation steps are complicated and the process is lengthy. It is very easy to introduce oxygen contamination, which increases the oxygen content in the finished plate (reaching 0.5% to 0.74%), thereby causing the mechanical strength and conductivity of the porous titanium diffusion layer to decrease. Therefore, exploring a reasonable and efficient method to successfully prepare a low-oxygen porous titanium diffusion layer has very important theoretical significance and practical application value. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide a method for preparing a porous titanium diffusion layer with a low oxygen content. The preparation method uses titanium powder with an oxygen mass percentage of 0.1% to 0.15% to roll a titanium thin strip green body, then places the titanium thin strip green body between a molybdenum plate and a zirconium oxide ceramic plate, and uses a stainless steel foil to cover it to prevent the titanium thin strip green body from contacting with oxygen during the sintering process, thereby preventing the oxygen content of the finished porous titanium diffusion layer from increasing. After vacuum sintering, a porous titanium diffusion layer with a low oxygen content is obtained, which solves the problem that the porous titanium diffusion layer prepared by the prior art has a high oxygen content, resulting in a decrease in the strength of the porous titanium diffusion layer.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a porous titanium diffusion layer with a low oxygen content, characterized in that the preparation method comprises the following steps:
[0006] Step 1, powder rolling: rolling titanium powder with an oxygen content of 0.1% to 0.15% by mass to form a titanium thin strip green body;
[0007] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, and then placing a molybdenum plate on the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure;
[0008] Step 3: Vacuum sintering: vacuum sintering the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 to obtain a porous titanium diffusion layer.
[0009] The present invention obtains a titanium thin strip green body by rolling titanium powder. Since the titanium thin strip green body is thin, low in strength and very easy to be damaged, a zirconia ceramic plate is provided to support the titanium thin strip green body to avoid damage to the titanium thin strip green body, and the zirconia will not react with the titanium thin strip green body to cause adhesion during the sintering process, thereby avoiding damage to the finished porous titanium diffusion layer; a molybdenum plate is placed on the titanium thin strip green body to keep the titanium thin strip green body in a spread state during the sintering process, thereby restraining the shrinkage of the titanium thin strip green body; at the same time, the titanium thin strip green body is placed between the molybdenum plate and the zirconia ceramic plate, so that the upper and lower surfaces of the titanium thin strip green body are respectively in close contact with the molybdenum plate and the zirconia ceramic plate, and then the titanium thin strip green body is sheathed to achieve isolation of the titanium thin strip green body from the environment in the sintering furnace, thereby reducing the probability of the titanium thin strip green body reacting with oxygen.
[0010] The above-mentioned method for preparing a porous titanium diffusion layer with low oxygen content is characterized in that the particle size of the titanium powder in step 1 is 20 μm to 50 μm, and the bulk density of the titanium powder is 0.8 g / cm 3 ~1.15g / cm 3 .
[0011] The above-mentioned method for preparing a porous titanium diffusion layer with a low oxygen content is characterized in that the rolling process in step 1 is: titanium powder is continuously fed between two counter-rotating rollers.
[0012] The present invention rolls a titanium thin strip blank by feeding titanium powder between two counter-rotating rollers. The technology extrude titanium powder particles by two rollers and utilizes the friction between the two rollers and the titanium powder, so that the titanium powder is fed between the rollers to be extruded and formed and then guided out by the friction. During preparation, the gap width between the two rollers can be adjusted according to the required thickness of the titanium thin strip blank to obtain titanium thin strip blanks of different thicknesses.
[0013] The above-mentioned method for preparing a porous titanium diffusion layer with low oxygen content is characterized in that the feeding speed is 10g / s to 60g / s, and the rotation speeds of the two rollers are both 3r / min to 12r / min.
[0014] The present invention controls the particle size and loose density of titanium powder, the titanium powder feeding speed and the roller rotation speed, thereby controlling the bite amount of titanium powder, so as to ensure that the titanium powder entering the gap between two rollers can be rolled into shape without breaking, and can control the thickness and density of the titanium thin strip green body. The porosity of the prepared titanium thin strip green body decreases as the density increases, thereby controlling the porosity of the porous titanium diffusion layer.
[0015] The above-mentioned method for preparing a low-oxygen content porous titanium diffusion layer is characterized in that the thickness of the molybdenum plate in step 2 is 0.1mm-0.5mm, the molybdenum plate completely covers the titanium thin strip green body, and the surface roughness Ra of the molybdenum plate is 10μm-40μm.
[0016] The present invention sets the thickness of the molybdenum plate to 0.1 mm to 0.5 mm and is able to completely cover the titanium thin strip green body, so as to ensure that the molybdenum plate has sufficient area and weight to constrain the titanium thin strip green body; by controlling the surface roughness Ra of the molybdenum plate to 10 μm to 40 μm, the friction between the molybdenum plate and the titanium thin strip green body is used to further constrain the titanium thin strip green body, so that the titanium thin strip green body will not shrink excessively during the formation and development of the sintering neck, thereby preventing the porosity of the porous titanium diffusion layer from being greatly reduced, and avoiding adhesion of different parts of the titanium thin strip green body, which affects the surface quality of the porous titanium diffusion layer.
[0017] The above-mentioned method for preparing a porous titanium diffusion layer with low oxygen content is characterized in that the vacuum sintering process in step 3 is: -2 Under the condition of Pa, the sheathed molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure is heated to 800°C-1100°C, then kept warm for 0.5h-2h, and cooled along with the furnace.
[0018] The above-mentioned method for preparing a porous titanium diffusion layer with a low oxygen content is characterized in that the mass percentage of oxygen element in the porous titanium diffusion layer in step three is 0.1% to 0.15%.
[0019] In addition, the present invention also discloses a porous titanium diffusion layer with low oxygen content, which is characterized in that it is obtained by the above preparation method.
[0020] The above-mentioned low-oxygen content porous titanium diffusion layer is characterized in that the porous titanium diffusion layer has a porosity of 20% to 40%, a thickness of 0.1 mm to 0.5 mm, a tensile strength of not less than 400 MPa, and an area of not less than 0.3 m 2 .
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] 1. The present invention controls the oxygen content of titanium powder to reduce the amount of oxygen introduced by the raw materials themselves, and places the titanium thin strip green body between the zirconium oxide ceramic plate and the molybdenum plate, and uses stainless steel foil for sheathing to prevent the titanium thin strip green body from contacting with oxygen during the sintering process, resulting in an increase in the oxygen content of the porous titanium diffusion layer, thereby realizing the preparation of a porous titanium diffusion layer with a low oxygen content.
[0023] 2. The present invention places the titanium thin strip green body between the zirconium oxide ceramic plate and the molybdenum plate to protect and constrain the titanium thin plate, control the titanium thin strip green body to always remain in a flat state, prevent the titanium thin strip green body from excessive shrinkage and adhesion during the sintering process, and ensure the porosity and surface quality of the porous titanium diffusion layer.
[0024] 3. The present invention controls the porosity and oxygen content of the porous titanium diffusion layer to achieve a tensile strength of not less than 400 MPa.
[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flow chart of the preparation method. DETAILED DESCRIPTION
[0027] Example 1
[0028] like Figure 1 As shown, the preparation method of this embodiment includes the following steps:
[0029] Step 1: Powder rolling: 323 g of powder with an oxygen content of 0.13%, a particle size of 22 μm to 30 μm, and a bulk density of 0.86 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 30 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 6 r / min;
[0030] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.3 mm, and the surface roughness Ra is 30 μm;
[0031] Step 3: Vacuum sintering: At a vacuum degree of 9.9×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 1050° C., kept warm for 1 hour and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0032] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.14%, a tensile strength of 436 MPa, a porosity of 29%, a thickness of 0.28 mm, and an area of 0.32 m 2 .
[0033] Example 2
[0034] The preparation method of this embodiment comprises the following steps:
[0035] Step 1: Powder rolling: 315 g of powder with an oxygen content of 0.11%, a particle size of 22 μm to 30 μm, and a bulk density of 0.86 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 30 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 6 r / min;
[0036] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.5 mm, and the surface roughness Ra is 30 μm;
[0037] Step 3: Vacuum sintering: At a vacuum degree of 9.9×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 1050° C., kept warm for 1 hour and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0038] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.15% by mass, a tensile strength of 407 MPa, a porosity of 36%, a thickness of 0.28 mm, and an area of 0.32 m 2 .
[0039] Example 3
[0040] The difference between this embodiment and embodiment 2 is that in step 1, the bulk density is 0.80 g / cm 3 of titanium powder.
[0041] After testing, the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.12% by mass, a tensile strength of 413 MPa, a porosity of 32%, a thickness of 0.26 mm, and an area of 0.32 m 2 .
[0042] Example 4
[0043] The preparation method of this embodiment comprises the following steps:
[0044] Step 1: Powder rolling: 436 g of powder with an oxygen content of 0.13%, a particle size of 26 μm to 44 μm, and a bulk density of 1.12 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 30 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 6 r / min;
[0045] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.5 mm, and the surface roughness Ra is 33 μm;
[0046] Step 3: Vacuum sintering: At a vacuum degree of 9.9×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 900° C., kept at this temperature for 1 hour, and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0047] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.13% by mass, a tensile strength of 439 MPa, a porosity of 23%, a thickness of 0.31 mm, and an area of 0.46 m 2 .
[0048] Example 5
[0049] The preparation method of this embodiment comprises the following steps:
[0050] Step 1: Powder rolling: 362 g of powder with an oxygen content of 0.10%, a particle size of 21 μm to 34 μm, and a bulk density of 0.88 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 30 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 6 r / min;
[0051] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally sheath the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.28 mm, and the surface roughness Ra is 29 μm;
[0052] Step 3: Vacuum sintering: At a vacuum degree of 2.9×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 1100° C., kept at this temperature for 0.5 h, and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0053] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.10%, a tensile strength of 487 MPa, a porosity of 23%, a thickness of 0.27 mm, and an area of 0.36 m 2 .
[0054] Example 6
[0055] The preparation method of this embodiment comprises the following steps:
[0056] Step 1: Powder rolling: 329 g of powder with an oxygen content of 0.15%, a particle size of 20 μm to 34 μm, and a bulk density of 1.13 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 33 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 8 r / min;
[0057] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.28 mm, and the surface roughness Ra is 27 μm;
[0058] Step 3: Vacuum sintering: At a vacuum degree of 2.7×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 1050° C., kept warm for 1 hour and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0059] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.15% by mass, a tensile strength of 403 MPa, a porosity of 31%, a thickness of 0.34 mm, and an area of 0.31 m 2 .
[0060] Example 7
[0061] The preparation method of this embodiment comprises the following steps:
[0062] Step 1: Powder rolling: 332 g of powder with an oxygen content of 0.12%, a particle size of 28 μm to 45 μm, and a bulk density of 1.10 g / cm 3The titanium powder is continuously fed into two counter-rotating rollers at a speed of 58 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 12 r / min;
[0063] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.49 mm, and the surface roughness Ra is 39 μm;
[0064] Step 3: Vacuum sintering: At a vacuum degree of 2.7×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 800°C, kept at this temperature for 2 hours and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0065] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.14%, a tensile strength of 426 MPa, a porosity of 39%, a thickness of 0.49 mm, and an area of 0.32 m 2 .
[0066] Example 8
[0067] The preparation method of this embodiment comprises the following steps:
[0068] Step 1: Powder rolling: 326 g of powder with an oxygen content of 0.11%, a particle size of 27 μm to 33 μm, and a bulk density of 0.92 g / cm 3 The titanium powder is continuously fed into two counter-rotating rollers at a speed of 35 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 5 r / min;
[0069] Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, placing a molybdenum plate on the titanium thin strip green body and completely covering the upper surface of the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally sheath the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; the thickness of the molybdenum plate is 0.12 mm, and the surface roughness Ra is 12 μm;
[0070] Step 3: Vacuum sintering: At a vacuum degree of 2.7×10 -2 Pa, the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 is heated to 1000° C., kept warm for 1 hour and then cooled with the furnace to obtain a porous titanium diffusion layer.
[0071] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.12% by mass, a tensile strength of 442 MPa, a porosity of 27%, a thickness of 0.12 mm, and an area of 0.32 m 2 .
[0072] Example 9
[0073] The difference between this embodiment and embodiment 8 is that in step 1, the particle size is 29 μm to 50 μm and the bulk density is 1.15 g / cm 3 Titanium powder is continuously fed into two counter-rotating rollers at a speed of 10 g / s for rolling to form a titanium thin strip green body; the rotation speed of the two rollers is 3 r / min.
[0074] The test results show that the porous titanium diffusion layer prepared in this embodiment has an oxygen content of 0.11%, a tensile strength of 467 MPa, a porosity of 30%, a thickness of 0.16 mm, and an area of 0.33 m 2 .
[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a porous titanium diffusion layer with low oxygen content, characterized in that: The preparation method comprises the following steps: Step 1, powder rolling: rolling titanium powder with an oxygen content of 0.1% to 0.15% by mass to form a titanium thin strip green body; Step 2, titanium thin strip green body tooling: placing the titanium thin strip green body formed in step 1 on a zirconia ceramic plate, and then placing a molybdenum plate on the titanium thin strip green body to form a molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure, and then using stainless steel foil to integrally cover the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure; Step 3: Vacuum sintering: vacuum sintering the molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure after the sheathing in step 2 to obtain a porous titanium diffusion layer.
2. The method for preparing a low oxygen content porous titanium diffusion layer according to claim 1, characterized in that: The particle size of the titanium powder in step 1 is 20 μm to 50 μm, and the bulk density of the titanium powder is 0.8 g / cm 3 ~1.15g / cm 3 .
3. The method for preparing a low oxygen content porous titanium diffusion layer according to claim 1, characterized in that: The rolling process described in step 1 is: titanium powder is continuously fed between two counter-rotating rollers.
4. The method for preparing a low oxygen content porous titanium diffusion layer according to claim 3, characterized in that: The feeding speed is 10 g / s to 60 g / s, and the rotation speeds of the two rollers are both 3 r / min to 12 r / min.
5. The method for preparing a low oxygen content porous titanium diffusion layer according to claim 1, characterized in that: In step 2, the thickness of the molybdenum plate is 0.1 mm to 0.5 mm, the molybdenum plate completely covers the titanium thin strip green body, and the surface roughness Ra of the molybdenum plate is 10 μm to 40 μm.
6. The method for preparing a porous titanium diffusion layer with low oxygen content according to claim 1, characterized in that: The vacuum sintering process in step 3 is as follows: the vacuum degree is not greater than 9.9×10 -2 Under the condition of Pa, the sheathed molybdenum plate-titanium thin strip green body-zirconia ceramic plate structure is heated to 800°C-1100°C, then kept warm for 0.5h-2h, and cooled along with the furnace.
7. The method for preparing a low oxygen content porous titanium diffusion layer according to claim 1, characterized in that: The oxygen content of the porous titanium diffusion layer in step 3 is 0.1% to 0.15% by mass.
8. A low oxygen content porous titanium diffusion layer, characterized in that: Obtained by the preparation method of any one of claims 1 to 7.
9. A low oxygen content porous titanium diffusion layer according to claim 8, characterized in that: The porous titanium diffusion layer has a porosity of 20% to 40%, a thickness of 0.1 mm to 0.5 mm, a tensile strength of not less than 400 MPa, and an area of not less than 0.3 m 2 .